Edge sealing device for tin bath of special float glass production line, preparation method and tin bath
By designing a combined edge sealing device of heat-resistant layer and thermal insulation layer on the tin tank of the special float glass production line, the structural strength and corrosion resistance of edge sealing in high-temperature and high-corrosion environment are solved, and good insulation and sealing are achieved The performance meets the requirements of the use of special glass production lines.
Patent Information
- Application Number
- CN202311461352.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-11-06
AI Technical Summary
The edge seal of ordinary float glass production lines is difficult to maintain structural strength under high temperature conditions of special float glass production lines, and is susceptible to volatiles in borosilicate glass mixing materials, resulting in insufficient insulation and sealing properties, which cannot meet high temperature and high corrosion. production requirements.
A tin tank edge sealing device for special float glass production line is designed, adopting a combined structure of heat-resistant layer and thermal insulation layer. The heat-resistant layer is close to the tin liquid, and the thermal insulation layer is far away from the tin liquid. The heat-resistant layer is composed of high-temperature refractory materials and contains Made of titanium austenitic stainless steel, the insulation layer is a high-density aluminum silicate fiber blanket, and a through-channel is provided between the inner box and the outer sealing plate to facilitate the operation of the forming auxiliary equipment.
Maintain good structural strength under ultra-high temperature conditions, improve corrosion resistance to volatile boron-containing compounds, enhance thermal insulation and sealing properties, extend the service life of the edge sealing device, and meet the production needs of special float glass production lines .
Smart Images

Figure CN117510043B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of float glass production equipment, and in particular relates to an edge sealing device for a tin bath of a special float glass production line, a preparation method and a tin bath. Background Art
[0002] When producing glass, various raw materials must first be mixed and made into a batch material, then the batch material is melted to form molten glass, and then the molten glass is cooled and formed into glass products. The formed glass products are then annealed to eliminate stress. Depending on the different processes in the forming stage, it can be divided into float glass, rolled glass, etc.
[0003] The forming process of ordinary float glass refers to the process of continuously passing the molten glass in the melting furnace into the tin bath filled with tin liquid at a temperature of about 1100℃ along the flow channel, and completing the forming process from the glass liquid to the glass original plate on the surface of the tin liquid. Since the density of the glass liquid is only about one-third of the density of the tin liquid, the glass liquid will float on the surface of the tin liquid with a relatively large density. When the glass liquid just flows into the tin bath, the temperature is high and the viscosity is low. Under the action of gravity and surface tension, it will spread and flatten on the tin liquid surface to form a glass ribbon, and then the thickness of the glass ribbon is controlled by the edge drawing machine in the high temperature zone. As the glass ribbon moves forward, the temperature of the glass ribbon gradually decreases and the viscosity gradually increases, and a glass original plate with uniform thickness is formed during the flow process. Therefore, the tin bath is a key thermal equipment for the formation of float glass.
[0004] The tin bath body includes a trough containing molten tin at the bottom, a large sealed cover at the top, and a gap between the trough and the cover; this gap can be used as a passage for forming auxiliary equipment such as edge drawing machines and water bags to enter and exit the tin bath, and is also an operating passage for handling tin bath accidents; in order to ensure the sealing and thermal insulation of the tin bath and meet the needs of normal production, the gaps on both sides of the tin bath need to be filled with edge seals, and the small gaps around the edge seals are then sealed with thermal insulation cotton and sealing putty.
[0005] The use of the side seals on both sides of the tin bath needs to meet the following requirements:
[0006] 1. The hot surface of the edge seal is exposed to the high temperature environment and atmosphere inside the tin bath. Therefore, the edge seal not only needs to have good structural strength under high temperature environment, but also needs to resist the corrosion of the atmosphere inside the tin bath. Therefore, the edge seal needs to be resistant to high temperature and corrosion;
[0007] 2. The edge seal needs to have strong thermal insulation performance to minimize the heat transfer from the tin bath to the external space, ensure the temperature in the tin bath is stable, and reduce the lateral temperature difference of the tin bath;
[0008] 3. The edge seal needs to have strong sealing performance to prevent external air from entering the tin bath, reduce tin liquid oxidation, and ensure stable atmosphere and pressure in the tin bath;
[0009] 4. The edge seal needs to reserve an operating hole or operating channel to meet the needs of forming auxiliary equipment entering the tin bath to work.
[0010] like Figure 1-3 As shown, the common edge seals used on both sides of the tin bath in the current common float glass production line generally consist of three parts: an outer sealing plate 4 outside the tin bath, an inner box body 5 inside the tin bath, and an insulation layer 6 inside the inner box body 5. The open end of the inner box body 5 is welded to the back of the outer sealing plate 4, and the outer sealing plate 4 and the inner box body 5 are generally made of heat-resistant stainless steel, which can withstand temperatures of about 900°C and has good corrosion resistance; the cross-section of the outer sealing plate 4 adopts a "C"-shaped structure, and a handle 7 is welded on the outer sealing plate 4 to facilitate the transportation, installation or disassembly of the edge seal; the material of the thermal insulation layer 6 is generally an aluminum silicate fiber blanket, which can play a good role in thermal insulation; gas exchange holes 8 are provided on the upper surface, lower surface, front surface and rear surface of the inner box body 5, which are convenient for the discharge of internal gas of the edge seal or the inflow of external air during the heating process of the tin bath or the disassembly of the edge seal, and prevent the inner box body 5 from bulging or sinking due to the thermal expansion and contraction of the gas in the inner box body 5. When the edge seal is made, an operating hole of corresponding shape can be reserved in the middle to facilitate the entry and exit of forming auxiliary equipment into the tin bath.
[0011] However, the melting and forming temperatures of special float glass production lines, such as high borosilicate glass production lines and TFT-LCD glass substrate production lines, are much higher than those of ordinary float glass production lines. The glass liquid temperature in the high-temperature zone at the upstream end of the tin bath can reach up to 1300-1400°C. According to actual production conditions, at such high temperatures, the inner box 5 of the ordinary edge seal will be less strong and prone to deformation. The aluminum silicate fiber blanket used in the insulation layer 6 will also melt, greatly reducing the thermal insulation of the edge seal. In addition, the boron compounds in the borosilicate glass batch components are volatile, and their volatiles are highly corrosive to the stainless steel inner box 4 of the ordinary edge seal exposed to the tin bath environment, reducing the service life of the edge seal. In summary, ordinary edge seals can no longer meet the production and use requirements of special float glass production lines. Summary of the invention
[0012] In view of the above-mentioned defects of the prior art, the present invention provides a side sealing device for a tin bath of a special float glass production line, a preparation method and a tin bath. The side sealing device can maintain good structural strength under the high temperature conditions of the special float glass production line, has stronger corrosion resistance to volatile boron-containing compounds in the borosilicate glass production line, and has good thermal insulation and sealing properties, thereby meeting the production and use requirements.
[0013] The technical solution adopted by the present invention to solve its technical problem is:
[0014] A side sealing device for a tin bath of a special float glass production line, the side sealing device being placed at the left gap and the right gap of the tin bath of the special float glass production line, and the side sealing device placed at the right gap of the tin bath, comprising an inner box body which is in the tin bath and has openings at both the left and right ends, the inner box body being provided with a plurality of gas exchange holes, a heat-resistant layer being provided in the left portion of the inner box body and a thermal insulation layer being provided in the right portion, the right side surface of the heat-resistant layer being tightly fitted with the left side surface of the thermal insulation layer, the outer peripheral surfaces of the heat-resistant layer and the thermal insulation layer being tightly fitted with the inner wall of the inner box body, the heat-resistant layer having a higher tolerance temperature than the thermal insulation layer, the heat-resistant layer being close to the tin liquid of the tin bath and the thermal insulation layer being far away from the tin liquid, the right end of the inner box body being sealed and fixedly connected with the left side surface of an outer sealing plate outside the tin bath; a through channel is also reserved on the heat-resistant layer and the thermal insulation layer, the through channel being connected with a through hole on the left side wall of the outer sealing plate, the through channel being matched with the through hole and being used as a channel for forming auxiliary equipment to enter and exit the tin bath.
[0015] Furthermore, the inner box body is assembled and welded by four heat-resistant stainless steel plates, and each of the heat-resistant stainless steel plates is provided with multiple gas exchange holes; the cross-section of the outer sealing plate is C-shaped and is made of heat-resistant stainless steel, the right end of the inner box body is sealed and welded to the left side of the outer sealing plate, and a handle is welded to the right part of the outer sealing plate.
[0016] Furthermore, the heat-resistant stainless steel plate of the inner box body is made of titanium-containing austenitic heat-resistant stainless steel with a thickness controlled at 2-3mm and a tolerance temperature controlled at 1000-1200°C, and the outer sealing plate is made of titanium-containing austenitic heat-resistant stainless steel with a thickness controlled at 3-4mm and a tolerance temperature controlled at 700-900°C.
[0017] Furthermore, a plurality of vertical heat-resistant stainless steel blocks are welded around the left edge of the inner box body, and the heat-resistant stainless steel blocks are located in the left end opening of the inner box body. The left side surface of the heat-resistant layer conflicts with the right side surface of each heat-resistant stainless steel block, and each heat-resistant stainless steel block cooperates and is used to prevent the heat-resistant layer from falling off.
[0018] Furthermore, the heat-resistant layer adopts a refractory material with a tolerance temperature greater than 1300°C, and the casting mud formed by mixing the casting material of the refractory material with water is used to cast into the left part of the inner box body, and is left to harden to form the heat-resistant layer; the insulation layer adopts a compression density greater than 220kg / m 3 an aluminum silicate fiber blanket; a heat-resistant stainless steel mesh is welded around the inner wall of the inner box at a position corresponding to the heat-resistant layer, and the horizontal width of the heat-resistant stainless steel mesh along the left and right directions is equal to the horizontal thickness of the heat-resistant layer along the left and right directions.
[0019] Furthermore, the castable composition of the refractory material is: 25-35wt% ZrO 2 15-20wt% SiO 2 , 0.5-1.5wt% Na 2 O, the rest is Al 2 O 3 .
[0020] Furthermore, the horizontal length of the inner box along the left-right direction is controlled within 200-400 mm, the horizontal length of the outer sealing plate along the left-right direction is controlled within 30-80 mm, and the horizontal thickness of the heat-resistant layer along the left-right direction is controlled within 10-100 mm.
[0021] Furthermore, a stainless steel shell with openings on both the left and right ends is welded on the left side surface of the outer sealing plate at the position of the through hole, the stainless steel shell extends into the through channel and the outer wall of the stainless steel shell is tightly fitted with the inner wall of the through channel, the cavity channel in the stainless steel shell cooperates with the through hole and serves as a channel for forming auxiliary equipment to enter and exit the tin bath, wherein the axis of the stainless steel shell is parallel to the axis of the inner box.
[0022] A method for preparing a tin bath edge sealing device for a special float glass production line, to prepare the tin bath edge sealing device for the special float glass production line, comprising the following steps:
[0023] S1. Assembling and welding four heat-resistant stainless steel plates to form the inner box, wherein each of the heat-resistant stainless steel plates is provided with a plurality of gas exchange holes;
[0024] S2. A heat-resistant layer is arranged in the left part of the inner box body, and the heat-insulating layer is arranged in the right part, wherein a through passage is reserved in the heat-resistant layer and the heat-insulating layer;
[0025] S3. Sealing and welding the right end of the inner box body to the left side surface of the outer sealing plate, and connecting the through channel to the through hole on the left side wall of the outer sealing plate to form the edge sealing device.
[0026] A tin bath for a special float glass production line comprises a bath containing molten tin at the bottom, a large sealed cover at the top, and a gap between the bath and the cover. The gap on the right side of the tin bath is provided with an edge sealing device for the tin bath of the special float glass production line, and the gap on the left side of the tin bath is provided with another edge sealing device symmetrical to the edge sealing device for the tin bath of the special float glass production line.
[0027] Compared with the prior art, the beneficial effects of the present invention are:
[0028] The edge sealing device for the tin bath of the special float glass production line of the present invention, wherein for the edge sealing device placed at the gap on the right side of the tin bath, since the heat-resistant layer arranged in the left part of the inner box body is close to the tin liquid in the tin bath, and the heat-insulating layer arranged in the right part of the inner box body is far away from the tin liquid in the tin bath, and the tolerance temperature of the heat-resistant layer is higher than that of the heat-insulating layer, the edge sealing device can withstand the ultra-high temperature in the tin bath of the special float glass production line and maintain good structural strength through the arrangement of the heat-resistant layer, and at the same time, the outer peripheral surface of the heat-resistant layer arranged in the left part of the inner box body and the inner part of the inner box body are close to each other. The heat-resistant layer is tightly fitted to the wall of the inner box, so that the heat-resistant layer supports the part of the inner box body with a higher temperature close to the tin liquid, so that the edge sealing device is not easy to deform when used at ultra-high temperatures, thereby ensuring the normal use of the forming auxiliary equipment that enters the tin bath through the through channel of the edge sealing device; in addition, since the left end of the inner box body is open, the heat-resistant layer arranged in the left part of the inner box body is directly in contact with the atmosphere inside the tin bath. For the high borosilicate glass production line, the heat-resistant layer of the edge sealing device is not easily affected by the highly corrosive and volatile boron-containing compounds, which can improve the The service life of the edge sealing device is improved; in addition, compared with the ordinary edge sealing in which the insulation layer is in the form of only a thin steel plate on the side close to the tin liquid of the tin bath, after the heat-resistant layer is added to the left side of the insulation layer, the heat transferred to the insulation layer is greatly reduced due to the heat-insulating effect of the heat-resistant layer, so the insulation layer is not easy to melt, so that the edge sealing device can meet the insulation conditions required by the tin bath of the special float glass production line. In addition, through the heat-insulating effect of the heat-resistant layer and the insulation layer, the overall thermal resistance of the edge sealing device is improved, which can reduce the heat dissipation; and in the production process, the heat-resistant layer and the insulation layer are used to make the edge sealing device have a better heat insulation performance. When making this edge sealing device, it is only necessary to set a heat-resistant layer in the left part of the inner box body and a thermal insulation layer in the right part, and reserve a through channel in the heat-resistant layer and the thermal insulation layer, and seal and fix the right end of the inner box body with the left side surface of the outer sealing plate, and make the through channel connected with the through hole on the left side wall of the outer sealing plate, so that the present edge sealing device can be formed. Therefore, the present edge sealing device is easy to make; in addition, the right side surface of the heat-resistant layer is tightly fitted with the left side surface of the thermal insulation layer, and the outer peripheral surfaces of the heat-resistant layer and the thermal insulation layer are tightly fitted with the inner wall of the inner box body, so that the sealing performance of the present edge sealing device is good.
[0029] In the present invention, a plurality of vertical heat-resistant stainless steel blocks are welded around the left edge of the inner box body, the heat-resistant stainless steel blocks are located in the left end opening of the inner box body, and the left side of the heat-resistant layer is in conflict with the right side of each heat-resistant stainless steel block; in this way, the cooperation of each heat-resistant stainless steel block can prevent the heat-resistant layer from falling off.
[0030] In the present invention, for the edge sealing device placed in the gap on the right side of the tin bath, the heat-resistant layer adopts a refractory material with a tolerance temperature greater than 1300°C, and a casting mud formed by mixing a casting material of the refractory material with water is used to be cast in the left part of the inner box body, and is left to harden to form a heat-resistant layer; in this way, for special float glass production lines such as high borosilicate glass production lines and TFT-LCD glass substrate production lines, the temperature of the glass liquid in the high-temperature zone at the upstream end of the tin bath can reach up to 1300-1400°C. The edge sealing device can withstand the ultra-high temperature in the tin bath of the special float glass production line and maintain good structural strength.
[0031] In the present invention, a heat-resistant stainless steel mesh is welded around the inner wall of the inner box at a position corresponding to the heat-resistant layer, and the horizontal width of the heat-resistant stainless steel mesh along the left and right directions is equal to the horizontal thickness of the heat-resistant layer along the left and right directions; the arrangement of the heat-resistant stainless steel mesh enables the castable used for the heat-resistant layer to be tightly combined with the inner wall of the inner box after hardening.
[0032] In summary, the edge sealing device can maintain good structural strength under the high temperature conditions of the special float glass production line, has stronger corrosion resistance to volatile boron-containing compounds in the borosilicate glass production line, and has good thermal insulation and sealing properties, meeting the production and use requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a three-dimensional structural schematic diagram of a common edge seal used in the gap on the right side of the tin bath in a common float glass production line in the background technology;
[0034] Figure 2 for Figure 1 A schematic diagram of a three-dimensional cross-sectional structure in another direction;
[0035] Figure 3 It is a schematic diagram of the main cross-sectional structure of a common edge seal used in the gap on the right side of the tin bath in a common float glass production line in the background technology;
[0036] Figure 4 It is a schematic diagram of the three-dimensional structure of the edge sealing device for the tin bath of the special float glass production line of the present invention when no through channel is reserved;
[0037] Figure 5 for Figure 4 A schematic diagram of a three-dimensional partial cross-sectional structure;
[0038] Figure 6 for Figure 5 A schematic diagram of the three-dimensional structure in another direction;
[0039] Figure 7 It is a three-dimensional structural schematic diagram of the case where the through passage reserved in the edge sealing device for the tin bath of the special float glass production line of the present invention is cylindrical;
[0040] Figure 8 for Figure 7 A schematic diagram of the three-dimensional structure in another direction;
[0041] Fig. 9 It is a schematic diagram of the three-dimensional structure when the through channel reserved in the edge sealing device for the tin bath of the special float glass production line of the present invention is in the shape of a rectangular parallelepiped;
[0042] Fig.10 for Fig. 9 A schematic diagram of the three-dimensional structure in another direction;
[0043] Fig.11 It is a schematic diagram of the main cross-sectional structure of the edge sealing device for the tin bath of the special float glass production line of the present invention when no through passage is reserved;
[0044] Fig.12 For Fig.11 Schematic diagram of the structure after dimensioning;
[0045] Fig.13 The present invention is a schematic diagram of a front cross-sectional structure in which an edge sealing device for a tin bath of a special float glass production line of the present invention is placed at the gap on the right side of the tin bath.
[0046] Explanation of the reference numerals in the figure: 1. Trough, 2. Large cover, 3. Edge sealing device, 4. Outer sealing plate, 5. Inner box, 6. Insulation layer, 7. Handle, 8. Gas exchange hole, 9. Heat-resistant layer, 10. Heat-resistant stainless steel mesh, 11. Heat-resistant stainless steel block, 12. Through channel, 13. Through hole. DETAILED DESCRIPTION
[0047] The specific embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings. These embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0048] In the description of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0049] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0050] Furthermore, in the description of the present invention, unless otherwise specified, “plurality” means two or more.
[0051] like Figure 4-11 As shown, a side sealing device for a tin bath of a special float glass production line, the side sealing device 3 is placed at the left gap and the right gap of the tin bath of the special float glass production line, and the side sealing device 3 placed at the right gap of the tin bath comprises an inner box body 5 which is in the tin bath and has openings at both the left and right ends, a plurality of gas exchange holes 8 are arranged on the inner box body 5, a heat-resistant layer 9 is arranged in the left part of the inner box body 5 and a heat-insulating layer 6 is arranged in the right part, the right side surface of the heat-resistant layer 9 is tightly fitted with the left side surface of the heat-insulating layer 6, and the heat-resistant layer 9 and The outer peripheral surface of the thermal insulation layer 6 is tightly fitted with the inner wall of the inner box 5, the heat-resistant layer 9 has a higher tolerance temperature than the thermal insulation layer 6, the heat-resistant layer 9 is close to the tin liquid in the tin bath and the thermal insulation layer 6 is far away from the tin liquid, and the right end of the inner box 5 is sealed and fixedly connected to the left side surface of the outer sealing plate 4 outside the tin bath; a through channel 12 is also reserved on the heat-resistant layer 9 and the thermal insulation layer 6, and the through channel 12 is connected to the through hole 13 on the left side wall of the outer sealing plate 4, and the through channel 12 cooperates with the through hole 13 and is used as a channel for forming auxiliary equipment to enter and exit the tin bath.
[0052] Since the heat-resistant layer 9 arranged in the left part of the inner box body 5 is close to the tin liquid in the tin bath, and the heat-insulating layer 6 arranged in the right part of the inner box body 5 is far away from the tin liquid in the tin bath, and the withstanding temperature of the heat-resistant layer 9 is higher than that of the heat-insulating layer 6, the edge sealing device 3 can withstand the ultra-high temperature in the tin bath of the special float glass production line and maintain good structural strength through the arrangement of the heat-resistant layer 9. At the same time, the outer peripheral surface of the heat-resistant layer 9 arranged in the left part of the inner box body 5 is tightly fitted with the inner wall of the inner box body 5, so that the heat-resistant layer 9 supports the part of the inner box body 5 with a higher temperature close to the tin liquid. The supporting effect makes it difficult for the edge sealing device 3 to deform when used at ultra-high temperatures, thereby ensuring the normal use of the forming auxiliary equipment that enters the tin bath through the through channel 12 of the edge sealing device 3; in addition, since the left end of the inner box body 5 is open, the heat-resistant layer 9 arranged in the left part of the inner box body 5 is directly in contact with the atmosphere inside the tin bath. For the high borosilicate glass production line, the heat-resistant layer 9 of the edge sealing device 3 is not easily affected by the corrosive and volatile boron-containing compounds, which can increase the service life of the edge sealing device 3; in addition, compared with the thermal insulation layer 6 in the ordinary edge seal, The side of the tin liquid close to the tin bath is in the form of only a thin steel plate. After the heat-resistant layer 9 is added to the left side of the thermal insulation layer 6, the heat transferred to the thermal insulation layer 6 is greatly reduced due to the thermal insulation effect of the heat-resistant layer 9. Therefore, the thermal insulation layer 6 is not easy to melt, so that the edge sealing device 3 can meet the thermal insulation conditions required by the tin bath of the special float glass production line. In addition, through the thermal insulation effect of the heat-resistant layer 9 and the thermal insulation layer 6, the overall thermal resistance of the edge sealing device 3 is improved, which can reduce the heat dissipation. Moreover, when manufacturing the edge sealing device 3, only the left side of the inner box body 5 needs to be provided. A heat-resistant layer 9 is arranged in the inner part and a thermal insulation layer 6 is arranged in the right part, and a through channel 12 is reserved in the heat-resistant layer 9 and the thermal insulation layer 6, and the right end of the inner box body 5 is sealed and fixedly connected with the left side surface of the outer sealing plate 4, and the through channel 12 is connected with the through hole 13 on the left side wall of the outer sealing plate 4, so that the edge sealing device 3 can be formed, so the edge sealing device 3 is easy to manufacture; in addition, the right side surface of the heat-resistant layer 9 is tightly fitted with the left side surface of the thermal insulation layer 6, and the outer peripheral surfaces of the heat-resistant layer 9 and the thermal insulation layer 6 are tightly fitted with the inner wall of the inner box body 5, so that the sealing performance of the edge sealing device 3 is good.
[0053] In one embodiment, the inner box body 5 is assembled and welded by four heat-resistant stainless steel plates. The inner box body 5 is in the shape of a rectangular tube as a whole. Each heat-resistant stainless steel plate is provided with a plurality of gas exchange holes 8. Figure 4-11 The gas exchange hole 8 is provided to facilitate the discharge of the gas inside the side seal or the inflow of outside air during the heating process of the tin bath or the removal of the side seal, so as to prevent the inner box body 5 from bulging or sinking due to the thermal expansion and contraction of the gas inside the inner box body 5; the cross section of the outer sealing plate 4 is C-shaped and made of heat-resistant stainless steel. The right end of the inner box body 5 is sealed and welded to the left side of the outer sealing plate 4, and a handle 7 is welded on the right part of the outer sealing plate 4. Figure 6 ,8 , 10 and 11, wherein the setting of the handle 7 facilitates the transportation, installation or disassembly of the edge sealing device 3.
[0054] In one embodiment,
[0055] The heat-resistant stainless steel plate of the inner box body 5 is made of titanium-containing austenitic heat-resistant stainless steel with a thickness controlled at 2-3mm and a withstand temperature controlled at 1000-1200°C. Preferably, the material of the inner box body 5 is 06Cr25Ni20; the outer sealing plate 4 is made of titanium-containing austenitic heat-resistant stainless steel with a thickness controlled at 3-4mm and a withstand temperature controlled at 700-900°C. Preferably, the outer sealing plate 4 is made of 06Cr18Ni11Ti with a thickness of 3mm; preferably, the horizontal length L1 of the inner box body 5 along the left and right direction is controlled at 200-400mm, and the horizontal length L2 of the outer sealing plate 4 along the left and right direction is controlled at 30-80mm, see Fig.12 .
[0056] The heat-resistant layer 9 is made of refractory material with a tolerance temperature greater than 1300°C. The casting mud formed by mixing the casting material of the refractory material with water is used to be cast in the left part of the inner box body 5, and is left to harden to form the heat-resistant layer 9. In this way, for special float glass production lines such as high borosilicate glass production lines and TFT-LCD glass substrate production lines, the glass liquid temperature in the high-temperature zone at the upstream end of the tin bath can reach up to 1300-1400°C. The edge sealing device 3 can withstand the ultra-high temperature in the tin bath of the special float glass production line and maintain good structural strength; the insulation layer 6 is made of a refractory material with a compression density greater than 220kg / m 3 Aluminum silicate fiber blanket.
[0057] like Figure 5 , 6 As shown in FIG. 11 , a heat-resistant stainless steel mesh 10 is welded around the inner wall of the inner box body 5 at a position corresponding to the heat-resistant layer 9, and the horizontal width of the heat-resistant stainless steel mesh 10 along the left-right direction is equal to the horizontal thickness of the heat-resistant layer 9 along the left-right direction. The arrangement of the heat-resistant stainless steel mesh 10 enables the castable used in the heat-resistant layer 9 to be tightly combined with the inner wall of the inner box body 5 after hardening.
[0058] The refractory castable material used in the heat-resistant layer 9 is composed of 25-35wt% ZrO 2 15-20wt% SiO 2 , 0.5-1.5wt% Na 2 O, the rest is Al 2 O 3 Preferably, the horizontal thickness d of the heat-resistant layer 9 along the left-right direction is controlled within 10-100 mm. Preferably, the horizontal thickness d of the heat-resistant layer 9 along the left-right direction is controlled within 30-60 mm. Fig.12 .
[0059] In one embodiment, Figure 4 , 5 As shown in FIGS. 6, 7, 9 and 11, a plurality of vertical heat-resistant stainless steel stoppers 11 are welded around the left edge of the inner box body 5. The heat-resistant stainless steel stoppers 11 are located in the left end opening of the inner box body 5, and the left side of the heat-resistant layer 9 is in conflict with the right side of each heat-resistant stainless steel stopper 11. In this way, the cooperation of each heat-resistant stainless steel stopper 11 can prevent the heat-resistant layer 9 from falling off.
[0060] In one embodiment, a stainless steel shell with openings on both the left and right ends is welded on the left side surface of the outer sealing plate 4 at the position of the through hole 13. The stainless steel shell extends into the through channel 12 and the outer wall of the stainless steel shell fits tightly with the inner wall of the through channel 12. The cavity channel in the stainless steel shell cooperates with the through hole 13 and serves as a channel for forming auxiliary equipment to enter and exit the tin bath. Preferably, the axis of the stainless steel shell coincides with the axis of the inner box body 5.
[0061] A method for preparing a tin bath edge sealing device for a special float glass production line, to prepare the tin bath edge sealing device for the special float glass production line, comprising the following steps:
[0062] S1, assembling and welding four heat-resistant stainless steel plates to form an inner box body 5, wherein each heat-resistant stainless steel plate is provided with a plurality of gas exchange holes 8;
[0063] S2. Pour the refractory castable material used for the heat-resistant layer 9 into a mixer, then gradually add an appropriate amount of water and stir until it becomes a sticky paste without stagnant water. Then pour the evenly stirred castable mud into the left part of the inner box 5 until the required horizontal thickness is reached. After standing for more than 24 hours, the hardened heat-resistant layer 9 is obtained, and the irregular parts in the heat-resistant layer 9 are modified and removed. After that, wait for natural air drying or place it in a high temperature environment to dry it to obtain the heat-resistant layer 9, and then fill the right part of the inner box 5 with a compression density greater than 220kg / m 3 Aluminum silicate fiber blanket is used to obtain a thermal insulation layer 6, wherein a through channel 12 is reserved in the heat-resistant layer 9 and the thermal insulation layer 6;
[0064] S3. A stainless steel shell with openings on both the left and right ends is seal-welded at the position of the through hole 13 on the left side of the outer sealing plate 4, and the stainless steel shell is extended into the through channel 12 reserved in the heat-resistant layer 9 and the thermal insulation layer 6, and the right end of the inner box body 5 is seal-welded to the left side of the outer sealing plate 4 to form an edge sealing device 3, in which the outer wall of the stainless steel shell is tightly fitted to the inner wall of the through channel 12.
[0065] like Fig.13As shown, a tin bath of a special float glass production line comprises a bath 1 containing molten tin at the bottom, a large sealed cover 2 at the top, and a gap between the bath 1 and the large cover 2. The gap on the right side of the tin bath is provided with the above-mentioned edge sealing device for the tin bath of the special float glass production line, which is used to seal the gap on the right side of the tin bath. The gap on the left side of the tin bath is provided with another edge sealing device which is symmetrical with the above-mentioned edge sealing device for the tin bath of the special float glass production line, which is used to seal the gap on the left side of the tin bath.
[0066] In summary, the edge sealing device 3 can maintain good structural strength under the high temperature conditions of the special float glass production line, has stronger corrosion resistance to volatile boron-containing compounds in the borosilicate glass production line, and has good thermal insulation and sealing properties, meeting the production and use requirements.
[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.
Claims
1. An edge sealing device for a tin bath of a special float glass production line, the edge sealing device (3) being arranged at the left gap and the right gap of the tin bath of the special float glass production line, with respect to the edge sealing device (3) arranged at the right gap of the tin bath, Features: The invention comprises an inner box body (5) which is located in a tin bath and has openings at both the left and right ends. The inner box body (5) is provided with a plurality of gas exchange holes (8). A heat-resistant layer (9) is provided in the left part of the inner box body (5) and a heat-insulating layer (6) is provided in the right part. The right side surface of the heat-resistant layer (9) is tightly fitted with the left side surface of the heat-insulating layer (6). The outer peripheral surfaces of the heat-resistant layer (9) and the heat-insulating layer (6) are tightly fitted with the inner wall of the inner box body (5). The heat-resistant layer (9) has a higher tolerance temperature than the heat-insulating layer. (6), the heat-resistant layer (9) is close to the tin liquid in the tin bath and the heat-insulating layer (6) is far away from the tin liquid, and the right end of the inner box (5) is sealed and fixedly connected to the left side surface of the outer sealing plate (4) outside the tin bath; a through channel (12) is also reserved on the heat-resistant layer (9) and the heat-insulating layer (6), and the through channel (12) is connected to the through hole (13) on the left side wall of the outer sealing plate (4), and the through channel (12) cooperates with the through hole (13) and serves as a channel for the forming auxiliary equipment to enter and exit the tin bath; The heat-resistant layer (9) is made of a refractory material with a tolerance temperature greater than 1300°C. The refractory material is mixed with water to form a casting mud, which is cast into the left part of the inner box (5) and left to harden to form the heat-resistant layer (9). A heat-resistant stainless steel mesh (10) is welded around the inner wall of the inner box (5) at a position corresponding to the heat-resistant layer (9). The horizontal width of the heat-resistant stainless steel mesh (10) in the left-right direction is equal to the horizontal thickness of the heat-resistant layer (9) in the left-right direction. The castable composition of the refractory material is: 25-35wt% ZrO 2 , 15-20wt% SiO 2 , 0.5-1.5wt% Na 2 O, the rest is Al 2 O 3 .
2. The edge sealing device for the tin bath of a special float glass production line according to claim 1, Features: The inner box body (5) is formed by assembling and welding four heat-resistant stainless steel plates, each of which is provided with a plurality of gas exchange holes (8); the outer sealing plate (4) has a C-shaped cross-section and is made of heat-resistant stainless steel; the right end of the inner box body (5) is sealed and welded to the left side of the outer sealing plate (4); and a handle (7) is welded to the right portion of the outer sealing plate (4).
3. The edge sealing device for the tin bath of a special float glass production line according to claim 2, Features: The heat-resistant stainless steel plate of the inner box body (5) is made of titanium-containing austenitic heat-resistant stainless steel with a thickness of 2-3 mm and a temperature resistance of 1000-1200° C., and the outer sealing plate (4) is made of titanium-containing austenitic heat-resistant stainless steel with a thickness of 3-4 mm and a temperature resistance of 700-900° C.
4. The edge sealing device for a tin bath of a special float glass production line according to claim 2, Features: A plurality of vertical heat-resistant stainless steel stoppers (11) are welded around the left edge of the inner box body (5), and the heat-resistant stainless steel stoppers (11) are located in the left end opening of the inner box body (5). The left side surface of the heat-resistant layer (9) abuts against the right side surface of each heat-resistant stainless steel stopper (11), and each heat-resistant stainless steel stopper (11) cooperates with and is used to prevent the heat-resistant layer (9) from falling off.
5. The edge sealing device for the tin bath of a special float glass production line according to claim 2, Features: The thermal insulation layer (6) has a compression density greater than 220 kg / m 3 Aluminum silicate fiber blanket.
6. The edge sealing device for the tin bath of a special float glass production line according to claim 2, Features: The horizontal length of the inner box body (5) along the left-right direction is controlled within a range of 200-400 mm, the horizontal length of the outer sealing plate (4) along the left-right direction is controlled within a range of 30-80 mm, and the horizontal thickness of the heat-resistant layer (9) along the left-right direction is controlled within a range of 10-100 mm.
7. The edge sealing device for the tin bath of a special float glass production line according to claim 2, Features: A stainless steel shell with openings on both the left and right ends is welded on the left side surface of the outer sealing plate (4) at the position of the through hole (13), the stainless steel shell extends into the through channel (12) and the outer wall of the stainless steel shell is tightly fitted with the inner wall of the through channel (12), the cavity channel in the stainless steel shell cooperates with the through hole (13) and serves as a channel for the forming auxiliary equipment to enter and exit the tin bath, wherein the axis of the stainless steel shell is parallel to the axis of the inner box body (5).
8. A method for preparing a tin bath edge sealing device for a special float glass production line, to prepare the tin bath edge sealing device for a special float glass production line as claimed in any one of claims 2 to 7, It is characterized in that The following steps are involved: S1, assembling and welding four heat-resistant stainless steel plates to form the inner box body (5), wherein each of the heat-resistant stainless steel plates is provided with a plurality of gas exchange holes (8); S2, arranging a heat-resistant layer (9) in the left part of the inner box body (5), and arranging the heat-insulating layer (6) in the right part, wherein a through passage (12) is reserved in the heat-resistant layer (9) and the heat-insulating layer (6); S3, sealingly welding the right end of the inner box body (5) to the left side surface of the outer sealing plate (4), and connecting the through channel (12) to the through hole (13) on the left side wall of the outer sealing plate (4), so as to form the edge sealing device (3).
9. A tin bath for a special float glass production line, comprising a bath (1) containing molten tin at the bottom, a large sealed cover (2) at the top, and a gap between the bath (1) and the cover (2). Features: The gap on the right side of the tin bath is provided with a side sealing device for the tin bath of a special float glass production line as claimed in any one of claims 2 to 7, and the gap on the left side of the tin bath is provided with another side sealing device (3) which is symmetrical with the side sealing device for the tin bath of a special float glass production line as claimed in any one of claims 2 to 7.