A kind of heat-stable high-toughness road cement concrete and preparation method thereof

By using carbon nanotubes to enhance the expanded vermiculite composite material and modified fibers and rubber powder in road cement concrete, the thermal stability and crack resistance of traditional cement concrete under high temperature conditions are solved, and high thermal stability and The improvement of crack resistance extends the service life of the road.

CN117510132BActive Publication Date: 2024-11-19JIANGSU CHINA CONSTR COMMERCIAL CONCRETE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311240996.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-25
Publication Date
2024-11-19
Estimated Expiration
2043-09-25

AI Technical Summary

Technical Problem

Traditional road cement concrete has poor thermal stability under high temperature conditions and poor bending and tensile crack resistance, resulting in cracks and damage, affecting the safety and durability of road use.

Method used

Using carbon nanotube-reinforced expanded vermiculite composite materials, modified sisal fibers, modified rubber powder and other components, through surface modification and modification treatment, road cement concrete with high thermal stability and excellent crack resistance is formed to enhance concrete Strength, toughness and crack resistance, and improve the mechanical properties and thermal conductivity of expanded vermiculite through carbon nanotubes.

Benefits of technology

The thermal stability and crack resistance of road cement concrete under high temperature conditions have been achieved, the concrete's load bending ability has been enhanced, the service life has been extended and safety has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004467287770000091
    Figure BDA0004467287770000091
  • Figure BDA0004467287770000101
    Figure BDA0004467287770000101
Patent Text Reader

Abstract

The invention discloses a thermally stable and high-toughness road cement concrete and a preparation method thereof, and belongs to the technical field of highway engineering. The concrete comprises the following components in parts by weight: 260-320 parts of cement, 20-30 parts of ceramic powder, 40-60 parts of fly ash, 1000-1100 parts of crushed stone, 450-480 parts of sand, 300-340 parts of carbon nanotube-reinforced expanded vermiculite composite material, 0.8-1.2 parts of modified sisal fiber, 3-6 parts of modified rubber powder, 5-7 parts of water reducer, and 160-170 parts of water. The invention coordinates a variety of materials with excellent thermal stability, crack resistance and toughness enhancement such as carbon nanotube-reinforced expanded vermiculite composite material, modified sisal fiber, modified rubber powder, ceramic powder, etc. Under the synergistic effect of each component, the road cement concrete of the invention has high thermal stability, high toughness and excellent crack resistance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of highway engineering, and in particular relates to a thermally stable and high-toughness road cement concrete and a preparation method thereof. Background Art

[0002] Cement concrete has developed into the most widely used engineering material in contemporary times due to its advantages such as wide source of raw materials, easy molding, strong adaptability and low cost. It is widely used in road paving and other fields. At present, cement pavement (grade highway) accounts for about 50% of the total mileage; therefore, cement pavement, as a major type of pavement structure, accounts for a considerable proportion in my country. However, traditional concrete has low tensile strength, and there is no obvious plastic deformation under load, and it suddenly breaks brittlely, and then cracks and breaks, which seriously affects the safety and durability of road cement concrete. Various studies have shown that the cracking caused by the high brittleness of concrete has become one of the main reasons for accelerating the corrosion and aging of concrete and causing damage to transportation infrastructure. Therefore, improving the tensile strength and toughness of road cement concrete plays an important role in improving the function and durability of road use.

[0003] Through the analysis of the road conditions of my country's road concrete in recent years, it is found that in the process of transportation, the amount of heavy and overloaded transportation has increased year by year, coupled with frequent hot weather in summer. Ordinary cement concrete pavement cannot withstand the coupling of multiple harsh working conditions such as large axle loads, high traffic flow and high temperatures in summer. It is very easy to break, stagger and lose air, and it is difficult to ensure normal use. Therefore, new road cement concrete materials must ensure that the concrete has sufficient strength, and must ensure that the concrete has a certain bending deformation ability and toughness. At the same time, it must also have the ability to resist high-temperature thermal expansion. Therefore, further improving the toughness of road cement concrete, making concrete develop in the direction of thermal stability, high toughness and low brittleness, and preparing high-durability and long-life cement concrete pavement is an important trend in the development of highway engineering. The compressive strength of ordinary concrete is much higher than the tensile strength. In order to effectively improve the toughness of concrete, the existing technology usually improves the brittleness of concrete by improving the concrete material itself, or by adding additives such as fiber, rubber, polymer, etc., thereby improving the flexural and tensile strength of concrete; however, the fiber toughness of conventional technical means is relatively poor, the flexural and tensile strength of concrete is limited, and it is difficult to evenly disperse in concrete, affecting the workability of concrete; there is poor compatibility and adhesion between rubber powder and cement, which leads to a weak interface transition zone between cement base and rubber powder, and the strength and hardness of concrete will be reduced. For example, Chinese patent CN111704405A discloses a sisal nanocellulose ultra-high toughness concrete and its preparation method, which is composed of the following components by mass percentage: 10% to 15% of silicate cement, 1.5% to 2% of fly ash, 2% to 5% of slag, 30% to 35% of fine aggregate, 44% to 48% of coarse aggregate, 0.1% to 0.2% of water reducer, and 0% to 0.1% of sisal nanocellulose. The ultra-high toughness concrete of this invention makes comprehensive use of two solid wastes, fly ash and slag, plus ultra-tough sisal nanocellulose. Under the action of water reducer, through reasonable mix design, the tensile properties of the prepared sisal nanocellulose ultra-high toughness concrete are far superior to ordinary concrete. At the same time, it can also improve the internal pore structure of the concrete and improve the durability of the concrete. However, this concrete does not take into account the improvement of thermal stability. Under high temperature conditions in summer, the temperature gradient inside the concrete will increase sharply, leading to thermal stress on the surface and inside of the concrete. This will then cause surface cracking and internal cracks, thereby damaging the integrity of the concrete.

[0004] In summary, it is of great significance to study how to enhance the toughness of road cement concrete while improving thermal stability, weaken the deterioration effects of the road caused by the coupling of load and high temperature environment during use, improve the durability of concrete such as crack resistance and fatigue resistance, reduce the occurrence of cracks, deformation and damage, and improve road safety and extend its service life. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, one of the objects of the present invention is to provide a thermally stable and high-toughness road cement concrete. Under the synergistic effect of various components, the road cement concrete of the present invention has high thermal stability, high toughness and excellent crack resistance, which solves the problems of poor thermal stability of traditional road cement concrete under high temperature conditions in summer and poor bending, tensile and crack resistance of concrete.

[0006] To achieve the above purpose, the specific technical solutions of the present invention are as follows:

[0007] A thermally stable and high-toughness road cement concrete comprises the following components in parts by weight: 260-320 parts of cement, 20-30 parts of ceramic powder, 40-60 parts of fly ash, 1000-1100 parts of crushed stone, 450-480 parts of sand, 300-340 parts of carbon nanotube reinforced expanded vermiculite composite material, 0.8-1.2 parts of modified sisal fiber, 3-6 parts of modified rubber powder, 5-7 parts of water reducer, and 160-170 parts of water;

[0008] The preparation method of the carbon nanotube reinforced expanded vermiculite composite material comprises the following steps:

[0009] The expanded vermiculite is soaked in a hydrochloric acid solution, washed and dried, and then soaked in a 3-aminopropyltrimethoxysilane solution, and dried to obtain the surface-modified expanded vermiculite;

[0010] The surface-modified expanded vermiculite is placed in a mixed solution of nickel nitrate and cobalt nitrate, immersed at 50-60° C. for 3-4 hours, and then vacuum dried; then, it is placed in a vapor deposition furnace, a carbon source is added under a protective gas atmosphere, and precipitated at 800-900° C. for 2-3 hours to obtain expanded vermiculite with carbon nanotubes grown on the surface;

[0011] The expanded vermiculite with carbon nanotubes grown on the surface is immersed in a KH-570 solution, taken out and dried to obtain the carbon nanotube-reinforced expanded vermiculite composite material.

[0012] Adding expanded vermiculite to concrete can enhance the flexural and tensile strength of concrete under high temperature conditions and improve its crack resistance. However, studies have shown that when the proportion of expanded vermiculite in fine aggregate exceeds 30%, the mechanical strength of concrete will be significantly reduced. The reason is that the particle size of expanded vermiculite is small and the interconnection between it and the cement matrix is ​​weak. A high proportion of incorporation will lead to more weaknesses and vulnerable parts, significantly reducing the mechanical properties of concrete. Carbon nanotubes have high strength, modulus, flexibility and thermal stability, but the dispersion of carbon nanotubes in the polymer matrix is ​​poor and cannot achieve the expected effect.

[0013] The present invention in-situ grows carbon nanotubes on the surface of expanded vermiculite, and the carbon nanotubes are fixed on the expanded vermiculite matrix. On the one hand, the problem of uneven dispersion of carbon nanotubes in concrete can be avoided, and the large specific surface area and rich microporous structure of the expanded vermiculite are helpful to provide more reaction interfaces, promoting the entry of carbon sources and the growth of carbon nanotubes; on the other hand, the introduction of carbon nanotubes effectively improves the relatively low mechanical properties of the expanded vermiculite, and the carbon nanotubes are fixed on the expanded vermiculite, and the expanded vermiculite becomes particles with countless tiny burrs, which effectively enhances the bite and adhesion of the expanded vermiculite to the cement matrix, and strengthens the strength, toughness and crack resistance of the road cement concrete; at the same time, the carbon nanotubes form a plurality of heat conduction tubes on the surface of the expanded vermiculite, which are helpful to reduce the temperature gradient inside the concrete and improve the thermal stability of the concrete under high temperature conditions; the carbon nanotube-reinforced expanded vermiculite composite material of the present invention can give full play to the complementary advantages of the expanded vermiculite and the carbon nanotubes, realize the use of a high amount of the expanded vermiculite, and make the prepared concrete have excellent thermal stability.

[0014] The carbon nanotube-reinforced expanded vermiculite composite material, sisal fiber and ceramic powder used in the concrete of the present invention are all materials with good thermal stability and are stable without expansion at high temperatures. At the same time, the carbon nanotubes and ceramic powder have high thermal conductivity. The high thermal conductivity enables them to effectively transfer heat, which helps the road concrete to evenly disperse the temperature downward, reduce the temperature gradient, reduce the risk of crack formation caused by local expansion, and enhance the ability of the road surface to resist load bending under high temperature conditions.

[0015] In the preparation method of the carbon nanotube reinforced expanded vermiculite composite material, 3-aminopropyltrimethoxysilane is used to modify the surface of the expanded vermiculite to improve its surface activity. At the same time, the amino group can form a coordination bond with the nickel-cobalt metal ions in the catalyst, thereby more effectively fixing it to the surface of the expanded vermiculite; the cobalt nitrate and nickel nitrate mixture is used as a catalyst to provide more active sites, increase the adsorption capacity of the carbon source, and promote the growth of carbon nanotubes; formaldehyde is easy to obtain, has high reactivity, and the carbon source generated after decomposition has high purity, which helps to effectively catalyze and promote the growth of carbon nanotubes , and prepare high-quality carbon nanotubes; finally, γ-methacryloxypropyltrimethoxysilane (KH-570) was used to wrap the expanded vermiculite. The trimethoxy part can form a stable silicon-oxygen bond with the hydroxyl group on the surface of the expanded vermiculite, firmly attached to the surface of the vermiculite and carbon nanotubes, and play a protective role; the γ-methacrylic part contains an unsaturated double bond, which can covalently react with the cement molecules in the concrete to form a bridging structure, improve the interfacial adhesion of the composite material, and further strengthen the close bonding between the carbon nanotube-reinforced expanded vermiculite composite material and the concrete.

[0016] Preferably, the modified sisal fiber is obtained by soaking the sisal fiber in a mixed solution of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water for 0.5 to 1.5 hours. More preferably, the mass ratio of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water is 1:(3 to 5):100.

[0017] Sisal fiber has the advantages of high tensile strength, strong toughness, good durability and thermal stability. When added to road cement concrete, it can form fine fiber tendons to aggregate and tie together the particles in the mortar, improve the aggregation and integrity of cement concrete, and reduce the deformation and expansion of concrete under high temperature conditions. In addition, sisal fiber can synergize with carbon nanotubes in carbon nanotube-reinforced expanded vermiculite composites to form a skeleton stacking reinforcement system in concrete. Sisal fiber forms a skeleton, and some carbon nanotubes scattered in the cement base connect and strengthen the tiny pores. Therefore, the addition of sisal fiber can enhance the overall stiffness, ductility and thermal stability of the concrete, and play a role in toughening and reducing the generation and development of cracks.

[0018] However, the diameter of sisal fiber is relatively large, and there will be certain gaps on the bonding surface with cement base, especially on the contact surface with aggregate. In addition, studies have shown that Ca(OH) 2 Crystallization in the inner cavity and pores of sisal fiber will make the sisal fiber brittle and gradually lose its reinforcing effect. The present invention uses poloxamer and 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide to modify sisal fiber. Poloxamer can improve the hydrophilicity of sisal fiber, improve the dispersion of fiber in concrete, and also improve the interfacial adhesion between sisal fiber and cement matrix; 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide can complex with calcium ions in cement to form a complex, which can fill the gaps caused by the contact between sisal fiber and cement-based bonding surface, especially aggregate surface, due to its large diameter, and reduce Ca(OH) 2 The tendency of crystallization in the inner cavity and pores of sisal fiber enables sisal fiber to fully play its toughening and strengthening role in concrete.

[0019] Preferably, the preparation method of the modified rubber powder comprises: soaking the rubber powder in an isopropanol aqueous solution for 1 to 1.5 hours, washing and drying, then soaking in a palmitamide solution for wetting treatment, then soaking in a polystyrene sulfonic acid solution for hydrophilic dispersion treatment, and drying to obtain the modified rubber powder. More preferably, the mass fraction of palmitamide in the palmitamide solution is 0.3% to 0.6%, and the mass fraction of polystyrene sulfonic acid in the polystyrene sulfonic acid solution is 1% to 2%; the soaking time for the wetting treatment is 30 to 60 minutes, and the soaking time for the hydrophilic dispersion treatment is 30 to 60 minutes.

[0020] Adding rubber powder to concrete can effectively inhibit the generation and development of concrete cracks, improve the ductility and load dissipation of road cement concrete, and also help improve thermal stability. However, the dispersibility of the rubber added in concrete and the adhesion to the cement base are poor, so the compressive strength and workability of the concrete will be reduced. The present invention utilizes isopropyl alcohol solution to remove impurities in the rubber powder and performs preliminary surface modification on the rubber powder. Palmitamide and polystyrene sulfonic acid solution are utilized to form a modification effect of first wetting and then hydrophilic dispersion on the rubber powder. Palmitamide has good wetting properties and can form a wetting layer on the surface of the rubber powder. Polystyrene sulfonic acid itself has excellent hydrophilicity and also acts as a dispersant. At the same time, the fatty acyl group of palmitamide can electrostatically interact with the sulfonic acid group in polystyrene sulfonic acid to form a soft film structure, which further enhances the hydrophilicity of the rubber powder after the wetting treatment, effectively improving the dispersibility, interface compatibility and bonding strength of the rubber powder in the cement matrix.

[0021] Preferably, the particle size of the ceramic powder is 1-40 μm, and the specific surface area is 500-600 m 2 / kg. Ceramic powder is rich in SiO 2 and Al 2 O 3 Chemical components such as Ca(OH) 2 The reaction forms calcium silicate hydrate, which fills the microscopic pores of concrete. At the same time, the fine ceramic powder can play a micro-aggregate effect, which can improve the compactness of concrete and reduce the shrinkage cracks of concrete. In addition, the ceramic powder has high thermal conductivity, which can better disperse and diffuse heat in concrete, reduce thermal stress concentration, and stabilize the overall structure.

[0022] Preferably, the content of carbon nanotubes in the carbon nanotube-reinforced expanded vermiculite composite material is 0.01 wt% to 0.03 wt%.

[0023] Preferably, the crushed stone is basalt with an apparent density of 2600-2700 kg / m 3 , crushing value ≤12%

[0024] Another object of the present invention is to provide a method for preparing the thermally stable and high-toughness road cement concrete, comprising the following steps:

[0025] S1. Weigh each component by weight;

[0026] S2. The modified rubber powder, ceramic powder, 1 / 4 water reducer and 1 / 4 water are mixed until uniform;

[0027] S3. Then add the cement, fly ash, sand, gravel, carbon nanotube-reinforced expanded vermiculite composite material, 2 / 4 of the water reducer and 2 / 4 of the water, mix well, then add the modified sisal fiber, the remaining 1 / 4 of the water reducer and 1 / 4 of the water, stir well to obtain a concrete slurry;

[0028] S5. After the concrete slurry is evenly mixed, it is put into the mold and placed on a vibration table for compaction for 20-30 seconds. After compaction, the surface is smoothed with a scraper. Under standard curing conditions, the mold is cured for 2 days before demolding.

[0029] In the preparation method of the present invention, step S2 first mixes the modified rubber powder particles and the ceramic powder, and the fine ceramic powder particles can first adhere to the rubber powder. The higher hardness and strength of the ceramic powder, combined with the flexibility and elasticity of the modified rubber powder, can promote the concrete to form a more excellent skeleton structure, improve the overall performance, effectively increase the tensile strength and crack resistance of the concrete, slow down and prevent the expansion of cracks, and improve the crack resistance of the concrete. In addition, after the dispersibility of the modified rubber powder is improved, the uniform distribution of the ceramic powder in the concrete matrix can be promoted, and while strengthening the combination and interaction of the ceramic powder with the cement matrix, the ceramic powder also fills the interface pores between the rubber powder and the cement base, and under the synergistic effect, the heat conduction, strength and crack resistance of the road cement concrete are further strengthened.

[0030] Compared with the prior art, the present invention is beneficial in that:

[0031] (1) The present invention directly grows carbon nanotubes in situ on the surface of expanded vermiculite, giving full play to the advantages of both, and realizing the use of large amounts of expanded vermiculite. On the one hand, expanded vermiculite provides more reaction interfaces for carbon nanotubes, which helps to promote the entry of carbon sources and the growth of carbon nanotubes, and effectively avoids the problem of uneven dispersion of carbon nanotubes in concrete. On the other hand, carbon nanotubes improve the interlayer performance of expanded vermiculite, improve the adhesion of expanded vermiculite to cement paste, and strengthen the strength, toughness and crack resistance of road cement concrete. Expanded vermiculite itself has excellent thermal stability, and carbon nanotubes form multiple heat conduction tubes on the surface of expanded vermiculite particles, which helps to reduce the temperature gradient inside the concrete, improve the heat conduction of road cement concrete under high temperature conditions, and enhance the ability of the road surface to resist load bending under high temperature conditions.

[0032] (2) The present invention uses poloxamer and 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide to modify sisal fiber, thereby improving the interfacial adhesion between sisal fiber and cement base and the dispersibility in concrete; 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide can react with cement and Ca(OH) 2The calcium ions in the sisal fiber can be complexed to form a complex, which can fill the gaps between the sisal fiber and the cement-based bonding surface, especially the aggregate surface, due to its large diameter. On the other hand, it can reduce the Ca(OH) 2 The tendency of crystallization in the inner cavity and pores of sisal fiber enables sisal fiber to fully play its toughening and strengthening role in concrete.

[0033] (3) The present invention utilizes palmitamide and polystyrene sulfonic acid solution to modify the rubber powder by first wetting it and then dispersing it hydrophilically, thereby enhancing the hydrophilicity of the rubber powder and effectively improving the dispersion performance, interface compatibility and bonding strength of the rubber powder in the cement matrix.

[0034] (4) The present invention coordinates a variety of materials with excellent thermal stability, crack resistance and toughness enhancement, such as carbon nanotube-reinforced expanded vermiculite composite materials, modified sisal fibers, modified rubber powder, and ceramic powder. While ensuring the strength of road cement concrete, the concrete's resistance to high-temperature thermal expansion, bending deformation capacity and toughness are fully improved. The road cement concrete of the present invention has a 28d compressive strength of ≥50MPa, a 28d flexural tensile strength of ≥8MPa, a thermal conductivity of ≤0.55W / m·K, an elongation of concrete at 100°C of ≤0.02%, and an early crack resistance flat plate test of the highest level V, which has the comprehensive characteristics of thermal stability, high toughness and crack resistance. DETAILED DESCRIPTION

[0035] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] In the following examples and comparative examples, the expanded vermiculite is prepared by heating and expanding raw vermiculite at high temperature, with a particle size of 20 to 30 meshes, and a thermal expansion coefficient of (1.4 to 1.6)×10 -5 / ℃; the diameter of carbon nanotubes in carbon nanotube-reinforced expanded vermiculite composite materials is 40-80nm and the length is 5-15μm; the ceramic powder is obtained by crushing waste ceramic tiles and grinding them in a cement test mill for 1-2h, with a particle size of 1-40μm and a specific surface area of ​​500-600m 2 / kg; the particle size of the modified rubber powder is 200-300 μm; the cement is ordinary Portland cement PO42.5; the particle size of the crushed stone (basalt) is 5-20 mm, and the crushing value is ≤12%; the sand (basalt) is prepared by dry machine-made sand technology, with a particle size of 0-5 mm and a fineness modulus of 2.7-3.0; the water reducer is a polycarboxylic acid high-performance water reducer with a water reduction rate of 22-28%; other raw materials used are commercially available products.

[0037] Example 1

[0038] The present embodiment provides a thermally stable and high-toughness road cement concrete, comprising the following components in parts by weight: 300 parts of cement, 20 parts of ceramic powder, 50 parts of fly ash, 1030 parts of crushed stone, 460 parts of sand, 320 parts of carbon nanotube reinforced expanded vermiculite composite material, 1.0 part of modified sisal fiber, 4 parts of modified rubber powder, 6 parts of water reducer, and 165 parts of water;

[0039] The preparation method of the carbon nanotube reinforced expanded vermiculite composite material comprises the following steps:

[0040] (1) soaking the expanded vermiculite in a dilute hydrochloric acid solution (1 wt%) to remove impurities, rinsing with deionized water, drying at 100° C. for 2 h, and then soaking in a 3-aminopropyltrimethoxysilane solution (0.8 wt%) for 20 to 30 min, stirring at a low speed during the soaking process, and obtaining surface-modified expanded vermiculite after drying;

[0041] (2) placing the surface-modified expanded vermiculite in a mixed solution of nickel nitrate and cobalt nitrate (the concentration of nickel nitrate in the mixed solution is 0.2 mol / L, and the concentration of cobalt nitrate is 1 mol / L), soaking it at 50°C for 4 hours, and then vacuum drying it; then placing it in a chemical vapor deposition furnace, using formaldehyde as a carbon source with a flow rate of 16 L / h, using argon as a protective gas with a flow rate of 1000 L / h, and precipitating it at 900°C for 2 hours, and finally placing it at 600°C for 3 hours under the protection of oxygen to remove unreacted carbon source and catalyst, thereby obtaining expanded vermiculite with carbon nanotubes grown on the surface;

[0042] (3) The expanded vermiculite with carbon nanotubes grown on the surface was placed in a KH-570 solution (0.8 wt%), immersed at 40° C. for 20 min, taken out and dried to a saturated surface dry state, to obtain a carbon nanotube-reinforced expanded vermiculite composite material.

[0043] The modified sisal fiber is obtained by immersing sisal fiber with a length of 10 to 15 mm in a mixed solution of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water for 1 hour, with continuous low-speed stirring during the immersion process. The mass ratio of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water in the mixed solution is 1:5:100.

[0044] The preparation method of modified rubber powder comprises the following steps: soaking the rubber powder in an isopropanol aqueous solution (isopropanol: water volume ratio = 1:1) for 1 hour, rinsing with deionized water and drying naturally; then soaking the rubber powder in a palmitamide solution (0.6wt%) for 30 minutes for wetting treatment, taking it out and soaking it in a polystyrene sulfonic acid solution (2wt%) for 30 minutes for hydrophilic dispersion treatment, and drying naturally to obtain the modified rubber powder.

[0045] The preparation method of the heat-stable high-toughness road cement concrete of the present embodiment comprises the following steps:

[0046] S1. Weigh each component by weight;

[0047] S2. Mix the modified rubber powder, ceramic powder, 1 / 4 water reducer and 1 / 4 water at a speed of 90 to 100 rpm for 60 to 90 seconds until the mixture is uniform;

[0048] S3. Then add cement, fly ash, sand, gravel, carbon nanotube-reinforced expanded vermiculite composite material, 2 / 4 water reducer and 2 / 4 water, and mix at a speed of 90 to 100 rpm for 40-60s; then add modified sisal fiber, the remaining 1 / 4 water and 1 / 4 water reducer, and continue stirring for 90s-120s to obtain a concrete slurry;

[0049] S5. After the slurry is stirred evenly, it is put into the mold and placed on a vibration table for compaction for 20-30 seconds. After compaction, the surface is smoothed with a scraper and cured for 2 days under standard curing conditions before demolding.

[0050] Note: 1 / 4 of water reducer refers to 1 / 4 of the total amount of water reducer, and 1 / 4 of water refers to 1 / 4 of the total amount of water.

[0051] Example 2

[0052] The heat-stable high-toughness road cement concrete of this embodiment is basically the same as that of Embodiment 1, except that it includes the following components in parts by weight: 260 parts of cement, 30 parts of ceramic powder, 60 parts of fly ash, 1000 parts of crushed stone, 450 parts of sand, 340 parts of carbon nanotube-reinforced expanded vermiculite composite material, 1.2 parts of modified sisal fiber, 6 parts of modified rubber powder, 5 parts of water reducer, and 170 parts of water;

[0053] The preparation method of the carbon nanotube reinforced expanded vermiculite composite material comprises the following steps:

[0054] (1) soaking the expanded vermiculite in a dilute hydrochloric acid solution (0.5 wt%) to remove impurities, rinsing with deionized water, drying at 70° C. for 4 h, and then soaking in a 3-aminopropyltrimethoxysilane solution (0.5 wt%) for 20 to 30 min, stirring at a low speed during the soaking process, and obtaining surface-modified expanded vermiculite after drying;

[0055] (2) placing the surface-modified expanded vermiculite in a mixed solution of nickel nitrate and cobalt nitrate (the concentration of nickel nitrate in the mixed solution is 0.2 mol / L, and the concentration of cobalt nitrate is 0.5 mol / L), soaking it at 60°C for 3 hours, and then vacuum drying it; then placing it in a chemical vapor deposition furnace, using formaldehyde as a carbon source with a flow rate of 12 L / h, using argon as a protective gas with a flow rate of 800 L / h, and precipitating it at 800°C for 3 hours, and finally placing it at 500°C for 4 hours under the protection of oxygen to remove unreacted carbon source and catalyst, thereby obtaining expanded vermiculite with carbon nanotubes grown on the surface;

[0056] (3) The expanded vermiculite with carbon nanotubes grown on the surface was placed in a KH-570 solution (0.5 wt%), immersed at 30° C. for 30 min, taken out and dried to a saturated surface dry state, to obtain a carbon nanotube-reinforced expanded vermiculite composite material.

[0057] The modified sisal fiber is obtained by immersing sisal fiber with a length of 10 to 15 mm in a mixed solution of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water for 1 hour, with continuous low-speed stirring during the immersion process. The mass ratio of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water in the mixed solution is 1:5:100.

[0058] The preparation method of modified rubber powder comprises the following steps: soaking the rubber powder in an isopropanol aqueous solution (isopropanol: water volume ratio = 1:1) for 1.5 hours, rinsing with deionized water and drying naturally; then soaking the rubber powder in a palmitamide solution (0.3wt%) for 50 minutes for wetting treatment, taking it out and soaking it in a polystyrene sulfonic acid solution (1.0wt%) for 50 minutes for hydrophilic dispersion treatment, and drying naturally to obtain the modified rubber powder.

[0059] Example 3

[0060] The heat-stable and high-toughness road cement concrete of this embodiment is basically the same as that of Example 1, except that it includes the following components in parts by weight: 320 parts of cement, 20 parts of ceramic powder, 40 parts of fly ash, 1100 parts of crushed stone, 480 parts of sand, 300 parts of carbon nanotube reinforced expanded vermiculite composite material, 0.8 parts of modified sisal fiber, 3 parts of modified rubber powder, 7 parts of water reducer, and 160 parts of water.

[0061] Comparative Example 1

[0062] The difference between Comparative Example 1 and Example 1 is that expanded vermiculite is used instead of the carbon nanotube reinforced expanded vermiculite composite material in Example 1.

[0063] Comparative Example 2

[0064] The difference between Comparative Example 2 and Example 1 is that unmodified sisal fiber is used instead of modified sisal fiber, and the amount used remains unchanged.

[0065] Comparative Example 3

[0066] The difference between Comparative Example 3 and Example 1 is that unmodified rubber powder is used instead of modified rubber powder, and the amount used remains unchanged.

[0067] Comparative Example 4

[0068] The difference between Comparative Example 4 and Example 1 is that an equal amount of fly ash is used to replace the ceramic powder.

[0069] The road cement concrete of Examples 1 to 3 and Comparative Examples 1 to 4 was tested for performance indicators such as working performance, mechanical properties, early crack resistance, thermal conductivity, and thermal expansion performance. The test results are shown in Table 1.

[0070] According to the provisions of GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", the working performance of the fresh concrete of the embodiment and the comparative example was tested; according to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Ordinary Concrete" and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", the mechanical properties and early crack resistance of the concrete were tested;

[0071] According to the provisions of GB / T 10294-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Insulating Materials - Hot Plate Method", the thermal conductivity of concrete was tested using the IMDRY3001-II Concrete Thermal Conductivity Tester. Two concrete slabs with a size of 300mm×300mm×30mm were used in the test, with the hot plate temperature set to 40℃ and the cold plate temperature set to 20℃.

[0072] The thermal expansion performance of concrete was tested with reference to the concrete length measurement method in the alkali aggregate reaction test in GB / T50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete". The specimen size is 25mm×25mm×280mm, and the pre-molding end is equipped with a triple test mold with a copper column head. The mold is removed after 1d of pouring (to ensure that the copper column head is intact when removing the mold) and cured for 28d under standard curing conditions. The specimen is then placed in a 60℃ oven for drying for 24h, taken out and cooled to room temperature, and its initial length is measured by a length ratio meter and then placed in a high-temperature furnace for heating. The test temperature is from 24℃±2℃ to 100℃, and the temperature rise rate is controlled to be 5℃ / mm. The specimen length, final elongation and average linear expansion coefficient of the specimen are recorded.

[0073] Table 1 Concrete performance test results

[0074]

[0075]

[0076] From the test results in Table 1, it can be seen that in terms of working performance, the slump of Examples 1 to 3 is more than 170mm, which has relatively good workability, and the water consumption is not significantly increased compared with conventional road cement concrete in terms of its mix ratio. During the test, the cohesiveness and water retention of the concrete of the present invention are good; in terms of mechanical properties, the 7d flexural tensile strength of Examples 1 to 3 is higher than 5.9MPa, which can meet the requirements of opening traffic on heavy traffic pavements (>5.5MPa), the 28d flexural tensile strength can reach about 1 / 7 of the 28d compressive strength, and the flexural tensile strength exceeds 8.0MPa, which has extremely excellent heavy-load flexural tensile performance; the early anti-crack flat plate test results show that the total cracking area per unit area of ​​Examples 1 to 3 is 35mm 2 / m 2 Within , there are almost no cracks visible to the naked eye on the appearance of the flat plate, and the concrete cracking grade belongs to the highest grade V, which shows that the concrete of the present invention has excellent crack resistance.

[0077] Compared with Example 1, Comparative Example 1 uses expanded vermiculite instead of carbon nanotubes to reinforce expanded vermiculite composite materials, and the slump of concrete is slightly greater than that of Example 1. This is because the components of Comparative Example 1 do not contain carbon nanotubes, which will reduce the working performance of concrete to a certain extent. In terms of mechanical properties, the 28d compressive strength and flexural tensile strength are reduced by 7.0MPa and 1.5MPa respectively compared with Example 1, and the total crack area per unit area is increased by 80mm 2 / m 2 This may be because a larger amount of expanded vermiculite will significantly reduce the strength of concrete. It also shows that the introduction of carbon nanotubes can ensure the use of a higher amount of expanded vermiculite, and at the same time can effectively improve the relatively low mechanical properties of expanded vermiculite. Carbon nanotubes are fixed on the expanded vermiculite, which effectively enhances the bite and adhesion of the expanded vermiculite to the cement matrix, and strengthens the strength, toughness and crack resistance of road cement concrete.

[0078] The sisal fiber of comparative example 2 was not modified, and the slump and 28d flexural strength of the concrete were 155mm and 7.1MPa respectively, and the total cracking area per unit area was 89mm 2 / m 2, which are lower than those in the embodiments, indicating that the modification of sisal fiber in the present invention can improve the interfacial adhesion between sisal fiber and cement base and the dispersibility in concrete, and sisal fiber plays a good toughening and strengthening role in concrete; the rubber powder in comparative example 3 is not modified, and the slump, 28d compressive strength, flexural tensile strength and early anti-cracking performance indicators of its concrete are lower than those in embodiments 1 to 3 to varying degrees, indicating that the modification effect of first wetting and then hydrophilic dispersion of rubber powder by palmitamide and polystyrene sulfonic acid solution is enhanced, and the hydrophilicity of rubber powder is enhanced, and the dispersibility, interfacial compatibility and bonding strength of rubber powder in cement matrix are effectively improved. After modification, the macroscopic test shows that the working mechanical properties and early anti-cracking performance of concrete are improved; comparative example 4 uses fly ash instead of ceramic powder. From the results of mechanical and anti-cracking performance tests, it can be seen that ceramic powder has better micro-aggregate effect than fly ash, improves the compactness of concrete, and reduces the occurrence of shrinkage cracks in concrete.

[0079] Thermal conductivity is an important factor affecting the thermal insulation of building materials. The smaller the thermal conductivity of a material, the better its thermal insulation performance and the stronger its heat preservation ability. By testing the thermal conductivity of concrete, it can be seen that the thermal conductivity of concrete in Examples 1 to 3 is generally less than 0.55, which is more than 80% lower than the thermal conductivity of conventional road cement concrete. Expanded vermiculite is a porous material. When added to concrete, it can increase the porosity inside the concrete to a certain extent. The micropores of expanded vermiculite are not interconnected, and the air inside it that does not circulate becomes a good insulating medium, which reduces the thermal conductivity of concrete. In addition, the thermal conductivity of each component material in the present invention is mostly lower than that of the component material of conventional road concrete. After equal volume substitution, the thermal conductivity of the prepared road cement concrete further decreases. From the test results of thermal expansion performance of concrete, compared with Example 1, the average linear thermal expansion coefficient of concrete in Comparative Example 1 and Comparative Example 4 increased by 11.8% and 14.6% respectively, and the thermal stability of concrete decreased significantly, which shows that the introduction of carbon nanotubes can form multiple heat conduction tubes on the surface of expanded vermiculite particles to a certain extent, which helps to reduce the temperature gradient inside the concrete, improve the thermal stability of road cement concrete under high temperature conditions, and reduce the expansion rate of concrete. Ceramic powder can better disperse and diffuse heat in concrete, reduce thermal stress concentration, stabilize the overall structure, and improve the thermal stability of concrete.

[0080] Based on the comprehensive test results, the present invention synergizes a variety of materials with excellent thermal stability, crack resistance and toughness enhancement properties, such as carbon nanotube-reinforced expanded vermiculite composite materials, modified sisal fibers, modified rubber powder, and ceramic powder. While ensuring the strength of road cement concrete, it also fully improves the concrete's resistance to high-temperature thermal expansion, bending deformation capacity and toughness. The prepared road cement has the comprehensive characteristics of thermal stability, high toughness, and crack resistance.

[0081] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A thermally stable and high-toughness road cement concrete, characterized in that: The invention comprises the following components in parts by weight: 260-320 parts of cement, 20-30 parts of ceramic powder, 40-60 parts of fly ash, 1000-1100 parts of crushed stone, 450-480 parts of sand, 300-340 parts of carbon nanotube reinforced expanded vermiculite composite material, 0.8-1.2 parts of modified sisal fiber, 3-6 parts of modified rubber powder, 5-7 parts of water reducer and 160-170 parts of water; The preparation method of the carbon nanotube reinforced expanded vermiculite composite material comprises the following steps: The expanded vermiculite is soaked in a hydrochloric acid solution, washed and dried, and then soaked in a 3-aminopropyltrimethoxysilane solution, and dried to obtain the surface-modified expanded vermiculite; The surface-modified expanded vermiculite is placed in a mixed solution of nickel nitrate and cobalt nitrate, immersed at 50-60°C for 3-4 hours, and then vacuum dried; then, it is placed in a vapor deposition furnace, a carbon source is added under a protective gas atmosphere, and precipitated at 800-900°C for 2-3 hours to obtain expanded vermiculite with carbon nanotubes grown on the surface; The expanded vermiculite with carbon nanotubes grown on the surface is immersed in a KH-570 solution, and the expanded vermiculite is taken out and dried to obtain the carbon nanotube-reinforced expanded vermiculite composite material; The modified sisal fiber is obtained by soaking the sisal fiber in a mixed solution of poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water for 0.5 to 1.5 hours; The preparation method of the modified rubber powder comprises: soaking the rubber powder in an isopropanol aqueous solution for 1 to 1.5 hours, washing and drying, then soaking the rubber powder in a palmitamide solution for wetting treatment, then soaking the rubber powder in a polystyrene sulfonic acid solution for hydrophilic dispersion treatment, and drying to obtain the modified rubber powder.

2. The heat-stable and high-toughness road cement concrete according to claim 1, characterized in that: The mass ratio of the poloxamer, 2,5-dihydroxy-N-(2-hydroxyethyl)benzamide and water is 1:(3-5):

100.

3. The heat-stable and high-toughness road cement concrete according to claim 1, characterized in that: The mass fraction of palmitamide in the palmitamide solution is 0.3% to 0.6%, and the mass fraction of polystyrene sulfonic acid in the polystyrene sulfonic acid solution is 1% to 2%.

4. The heat-stable and high-toughness road cement concrete according to claim 1, characterized in that: The immersion time for wetting treatment is 30~60min, and the immersion time for hydrophilic dispersion treatment is 30~60min.

5. The heat-stable and high-toughness road cement concrete according to claim 1, characterized in that: The particle size of the ceramic powder is 1-40 μm, and the specific surface area is 500-600 m 2 / kg.

6. The heat-stable and high-toughness road cement concrete according to claim 1, characterized in that: The content of carbon nanotubes in the carbon nanotube-reinforced expanded vermiculite composite material is 0.01 wt % to 0.03 wt %.

7. The heat-stable and high-toughness road cement concrete according to claim 1, characterized in that: The crushed stone is basalt with an apparent density of 2600-2700 kg / m 3 , crushing value ≤12%.

8. The method for preparing a heat-stable and high-toughness road cement concrete according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Weigh each component by weight; S2. The modified rubber powder, ceramic powder, 1 / 4 water reducer and 1 / 4 water, mixed until uniform; S3. Then add the cement, fly ash, sand, gravel, carbon nanotube-reinforced expanded vermiculite composite material, 2 / 4 of the water reducer and 2 / 4 of the water, mix well, then add the modified sisal fiber, the remaining 1 / 4 of the water reducer and 1 / 4 of the water, stir well to obtain a concrete slurry; S5. After the concrete slurry is evenly mixed, it is put into the mold and placed on a vibration table for compaction for 20-30 seconds. After compaction, the surface is smoothed with a scraper. Under standard curing conditions, the mold is cured for 2 days before demolding.