Methods to reduce oxygen content in molten steel

By controlling the carbon-oxygen balance and adding carbon-containing substances during the converter smelting and RH decarburization stages, the problem of high oxygen content in molten steel during low-carbon steel production was solved, achieving the effects of reducing deoxidized aluminum consumption and improving the cleanliness of molten steel.

CN117512265BActive Publication Date: 2026-11-17PANGANG GRP XICHANG STEEL & VANADIUM CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311650456.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-05
Publication Date
2026-11-17
Estimated Expiration
2043-12-05

AI Technical Summary

Technical Problem

In existing technologies, when producing low-carbon steel using converter smelting + RH decarburization process, the high oxygen content in the molten steel leads to a large consumption of deoxidized aluminum, poor cleanliness of the molten steel, and severe blockage of the sprue during the casting process, which affects the steady-state casting of continuous casting.

Method used

By controlling the oxygen content of molten steel during tapping based on the carbon-oxygen product at the end of the converter smelting stage, and combining the initial carbon and oxygen content during the RH decarburization stage, carbon-containing substances, including carbon-containing manganese alloys and carbon raisers, are added in batches at intervals to control the oxygen content of molten steel at a low level after RH decarburization.

Benefits of technology

Reduce the oxygen content of molten steel after RH decarburization, reduce the amount of deoxidized aluminum used, improve the cleanliness of molten steel, and avoid adverse effects on the casting process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for reducing the oxygen content of molten steel, comprising: during the converter smelting stage, controlling the oxygen content of the molten steel during tapping to a predetermined range based on the carbon-oxygen product of the molten steel at the converter endpoint; and during the RH decarburization stage, when the initial oxygen content of the molten steel entering the RH decarburization station is greater than the initial carbon content, adding carbonaceous substances to the molten steel for deoxidation. This invention can control the oxygen content of the molten steel to a low level after RH decarburization, thereby reducing the amount of aluminum used in the RH decarburization process, improving the cleanliness of the molten steel, and avoiding adverse effects on the casting process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of steelmaking technology, and more specifically to a method for reducing the oxygen content of molten steel. Background Technology

[0002] In the smelting of low-carbon steel (e.g., low-carbon steel with a carbon content of less than or equal to 0.06 wt%), a converter smelting + RH decarburization process is typically used. After RH decarburization, deoxidizing aluminum is often added to control the oxygen content of the molten steel within the target range. However, in existing technologies, the oxygen content of the molten steel is high at the end of the converter process and remains high after RH decarburization, resulting in high consumption of deoxidizing aluminum, poor steel cleanliness, severe nozzle blockage during casting, and affecting steady-state casting in continuous casting. Summary of the Invention

[0003] The main objective of this invention is to provide a method for reducing the oxygen content of molten steel, so as to solve the problems in the prior art where excessively high oxygen activity in molten steel leads to large consumption of deoxidized aluminum, poor cleanliness of molten steel, and affects the casting process.

[0004] According to one aspect of the present invention, a method for reducing the oxygen content of molten steel is provided, comprising:

[0005] During the converter smelting stage, the oxygen content of the molten steel is controlled within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the end of the converter process.

[0006] During the RH decarburization stage, when the initial oxygen content of the molten steel entering the RH station is greater than the initial carbon content, carbonaceous substances are added to the molten steel for deoxidation.

[0007] According to one embodiment of the present invention, controlling the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the converter endpoint includes:

[0008] When the carbon-oxygen product of the molten steel at the end of the converter is less than or equal to 0.0020%, the oxygen content of the molten steel during tapping should be controlled at 350-450 ppm.

[0009] According to one embodiment of the present invention, controlling the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the converter endpoint includes:

[0010] When the carbon-oxygen product of the molten steel at the end of the converter is greater than 0.0020% and less than or equal to 0.0025%, the oxygen content of the molten steel during tapping should be controlled at 450-550 ppm.

[0011] According to one embodiment of the present invention, controlling the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the converter endpoint includes:

[0012] When the carbon-oxygen product of the molten steel is greater than 0.0025% at the end of the converter process, the oxygen content of the molten steel should be controlled at 550-650 ppm during tapping.

[0013] According to one embodiment of the present invention, controlling the oxygen content of molten steel within a predetermined range during the tapping process includes:

[0014] When the oxygen content of the molten steel exceeds the upper limit of the predetermined range at the end of the converter process, a carburizing agent is added during the tapping process to deoxidize the steel, so that the oxygen content of the molten steel is within the predetermined range during the tapping process.

[0015] According to one embodiment of the present invention, controlling the oxygen content of molten steel within a predetermined range during the tapping process includes:

[0016] When the oxygen content of the molten steel is within the predetermined range at the end of the converter process, no carburizing agent is added during tapping.

[0017] According to one embodiment of the present invention, in the RH decarburization stage, when the initial oxygen content of the molten steel entering the RH station is less than the initial carbon content, natural decarburization is carried out.

[0018] According to one embodiment of the present invention, the carbon-containing substance is added starting 1.5 to 2 minutes after the RH treatment begins.

[0019] According to one embodiment of the present invention, the carbon-containing material includes a carbon-containing manganese alloy and a carbon raiser.

[0020] According to one embodiment of the present invention, the carbon-containing manganese alloy is added all at once, and the carbon raiser is added in batches at intervals.

[0021] In the technical solution of this invention, the carbon-oxygen balance of the molten steel at the converter source is first controlled. Based on the carbon-oxygen product of the molten steel at the converter end, the oxygen content of the molten steel during tapping is initially controlled within a suitable range. Then, in the RH decarburization stage, the initial carbon and initial oxygen contents of the molten steel entering the RH station are controlled again. When the initial oxygen content is too high, carbon-containing substances are added for deoxidation. Thus, through two controls, the oxygen content of the molten steel after RH decarburization is finally controlled at a low level. This can reduce the amount of aluminum used in the RH, improve the cleanliness of the molten steel, and avoid adverse effects on the casting process. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples.

[0023] It should be noted that all uses of "first" and "second" in the embodiments of the present invention are for the purpose of distinguishing two entities or parameters with the same name but different names. It is clear that "first" and "second" are only for the convenience of expression and should not be construed as limiting the embodiments of the present invention. Subsequent embodiments will not explain this in detail.

[0024] This invention proposes a method for reducing the oxygen content of molten steel, comprising:

[0025] During the converter smelting stage, the oxygen content of the molten steel is controlled within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the end of the converter process.

[0026] During the RH decarburization stage, when the initial oxygen content of the molten steel entering the RH station is greater than the initial carbon content (when comparing, the initial oxygen content and the initial carbon content are in the same unit), carbonaceous substances are added to the molten steel for deoxidation.

[0027] In an embodiment of the present invention, carbon-oxygen balance control is first performed on the molten steel at the converter source. Based on the carbon-oxygen product of the molten steel at the converter endpoint, the oxygen content of the molten steel during tapping is initially controlled within a suitable range. Then, during the RH decarburization stage, the initial carbon and initial oxygen contents of the molten steel entering the RH station are controlled again. When the initial oxygen content is too high, carbon-containing substances are added for deoxidation. Thus, through two controls, the oxygen content of the molten steel after RH decarburization is finally controlled at a low level. This can reduce the amount of aluminum used in the RH, improve the cleanliness of the molten steel, and avoid adverse effects on the casting process.

[0028] The inventors of this application recognize that the final carbon-oxygen product achievable by converters at different furnace ages varies, and increases with furnace age. For example, some combined blowing converters with less than 5000 heats of service life can achieve a final carbon-oxygen product of less than 0.0025%. As furnace age increases, the slag layer covering the surface of the permeable elements thickens, and the carbon-oxygen product may exceed 0.0030%. The inventors further recognize that the oxygen content of the molten steel increases to some extent after tapping. The larger the final carbon-oxygen product, the smaller the increase in oxygen content after tapping. Therefore, it is necessary to control the oxygen content differently based on the final carbon-oxygen product at different furnace ages. For converters with lower final carbon-oxygen products, the increase in oxygen content after tapping is larger, so the oxygen content in the molten steel during tapping needs to be controlled at a lower level. For converters with higher final carbon-oxygen products, the increase in oxygen content after tapping is smaller, so the oxygen content in the molten steel can be kept at a higher level during tapping. In other words, in the embodiments of the present invention, the smaller the carbon-oxygen product of the molten steel at the end of the converter process, the lower the oxygen content of the molten steel is controlled during tapping. The following is a detailed description of different scenarios:

[0029] In some embodiments, controlling the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the converter endpoint includes:

[0030] When the carbon-oxygen product of the molten steel at the end of the converter is less than or equal to 0.0020%, the oxygen content of the molten steel during tapping should be controlled at 350-450 ppm.

[0031] In some embodiments, controlling the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the converter endpoint includes:

[0032] When the carbon-oxygen product of the molten steel at the end of the converter is greater than 0.0020% and less than or equal to 0.0025%, the oxygen content of the molten steel during tapping should be controlled at 450-550 ppm.

[0033] In some embodiments, controlling the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the converter endpoint includes:

[0034] When the carbon-oxygen product of the molten steel is greater than 0.0025% at the end of the converter process, the oxygen content of the molten steel should be controlled at 550-650 ppm during tapping.

[0035] In some embodiments, controlling the oxygen content of the molten steel within a predetermined range during the tapping process includes:

[0036] When the oxygen content of the molten steel exceeds the upper limit of the predetermined range at the end of the converter process, a carburizing agent is added during the tapping process to deoxidize the steel, so that the oxygen content of the molten steel is within the predetermined range during the tapping process.

[0037] In some embodiments, controlling the oxygen content of the molten steel within a predetermined range during the tapping process includes:

[0038] When the oxygen content of the molten steel is within the predetermined range at the end of the converter process, no carburizing agent is added during tapping.

[0039] Relevant testing instruments can be used to measure the carbon-oxygen product and oxygen content of molten steel at the converter endpoint. Based on the measured carbon-oxygen product value at the endpoint, a corresponding predetermined range is determined. Then, the measured oxygen content at the endpoint is compared with the predetermined range to determine whether a recarburizing agent needs to be added for deoxidation. If it is determined that a recarburizing agent needs to be added, the amount of recarburizing agent to be added is further determined based on the oxygen content at the endpoint and the predetermined range. Finally, the oxygen content of molten steel during tapping is controlled within the predetermined range.

[0040] In some embodiments, during the RH decarburization stage, natural decarburization is performed when the initial oxygen content of the molten steel entering the RH station is less than the initial carbon content.

[0041] In some embodiments, the carbon-containing material is added starting 1.5 to 2 minutes after the RH treatment begins.

[0042] In some embodiments, the carbon-containing material includes a carbon-manganese alloy and a carbon raiser. Using a carbon-manganese alloy provides the required manganese content in the finished steel and allows for deoxidation through the carbon content. For example, the carbon-manganese alloy can be high-carbon ferromanganese. The amount of carbon-manganese alloy added can be determined based on the manganese content of the finished steel, and the amount of carbon raiser added can be determined based on the required amount of carbon supplementation. The carbon raiser can be any conventionally used carbon raiser, including but not limited to: anthracite carbon raisers, petroleum coke carbon raisers, metallurgical coke carbon raisers, graphite carbon raisers, etc.

[0043] In some embodiments, the carbon raiser is added in batches at intervals. For example, the carbon raiser can be added in batches of 30 kg, with a 30-second interval between each batch. Adding it in batches at intervals avoids the problem of an overly violent reaction. Carbon-manganese alloys, on the other hand, can be added all at once.

[0044] In summary, to address the issue of high oxygen content after RH decarburization in the production of low-carbon and micro-carbon steel using the RH process, this invention provides a feasible control method by controlling the carbon-oxygen balance at the converter source. Then, during the RH decarburization stage, based on the initial carbon content, initial oxygen content, and target carbon content of the molten steel entering the RH station, combined with the vacuum decarburization rate, this method utilizes low-cost carbon-manganese alloys and carbon-based composite materials to control the oxygen content of the molten steel at a low level (e.g., below 65 ppm) after RH decarburization. This reduces the amount of deoxidizing aluminum used subsequently and improves the cleanliness of the molten steel.

[0045] The following description is based on specific embodiments.

[0046] Example 1

[0047] The production process of low-carbon steel is controlled according to the following methods:

[0048] During the converter smelting stage, the carbon-oxygen product of the molten steel at the converter endpoint was measured to be 0.0017%. Since 0.0017% is less than 0.0020%, it is necessary to control the oxygen content of the molten steel during tapping to be between 350 and 450 ppm. The oxygen content of the molten steel at the converter endpoint was measured to be within this range. Therefore, no carburizing agent was added for deoxidation during the tapping process, and the oxygen content of the molten steel during tapping was 377 ppm.

[0049] During the RH decarburization stage, the initial oxygen content of the molten steel entering the RH station was measured to be 480 ppm, and the initial carbon content was 300 ppm. Since the initial oxygen content was greater than the initial carbon content, carbonaceous substances needed to be added to the molten steel for deoxidation. In this embodiment, the target carbon content was 200 ppm. Based on this target carbon content, 31 kg of anthracite recarburizing agent and 480 kg of high-carbon ferromanganese were added. Specifically, the anthracite recarburizing agent and high-carbon ferromanganese were added 1.7 minutes after the start of the RH treatment. The high-carbon ferromanganese was added all at once, while the anthracite recarburizing agent was added in batches of 30 kg, with a 30-second interval between each batch.

[0050] This embodiment reduces the oxygen content of molten steel to 30 ppm after RH decarburization.

[0051] Example 2

[0052] The production process of low-carbon steel is controlled according to the following methods:

[0053] During the converter smelting stage, the carbon-oxygen product of the molten steel at the converter endpoint was measured to be 0.0022%. Since 0.0022% is greater than 0.0020% but less than 0.0025%, it is necessary to control the oxygen content of the molten steel during tapping to be between 450 and 550 ppm. The oxygen content of the molten steel at the converter endpoint was measured to be greater than 550 ppm. Therefore, 81 kg of anthracite carbon raiser was added during the tapping process to deoxidize the steel, so that the oxygen content of the molten steel during tapping was 550 ppm.

[0054] During the RH decarburization stage, the initial oxygen content of the molten steel entering the RH station was measured to be 506 ppm, and the initial carbon content was 350 ppm. Since the initial oxygen content was greater than the initial carbon content, carbonaceous substances needed to be added to the molten steel for deoxidation. In this embodiment, the target carbon content was 220 ppm. Based on this target carbon content, 82 kg of anthracite recarburizing agent and 531 kg of high-carbon ferromanganese were added. The anthracite recarburizing agent and high-carbon ferromanganese were added starting 1.6 minutes after the RH treatment began. The high-carbon ferromanganese was added all at once, while the anthracite recarburizing agent was added in batches of 30 kg, with a 30-second interval between each batch.

[0055] This embodiment reduces the oxygen content of molten steel to 63 ppm after RH decarburization.

[0056] Example 3

[0057] The production process of low-carbon steel is controlled according to the following methods:

[0058] During the converter smelting stage, the carbon-oxygen product of the molten steel at the converter endpoint was measured to be 0.0028%. Since 0.0028% is greater than 0.0025%, it is necessary to control the oxygen content of the molten steel during tapping to be between 550 and 650 ppm. The oxygen content of the molten steel at the converter endpoint was measured to be greater than 650 ppm. Therefore, 32 kg of anthracite carbon raiser was added during the tapping process to deoxidize the steel, so that the oxygen content of the molten steel during tapping was 569 ppm.

[0059] During the RH decarburization stage, the initial oxygen content of the molten steel entering the RH station was measured to be 530 ppm, and the initial carbon content was 320 ppm. Since the initial oxygen content was greater than the initial carbon content, carbonaceous substances needed to be added to the molten steel for deoxidation. In this embodiment, the target carbon content was 220 ppm. Based on this target carbon content, 88 kg of anthracite recarburizing agent and 525 kg of high-carbon ferromanganese were added. The anthracite recarburizing agent and high-carbon ferromanganese were added 1.5 minutes after the start of the RH treatment. The high-carbon ferromanganese was added all at once, while the anthracite recarburizing agent was added in batches of 30 kg, with a 30-second interval between each batch.

[0060] This embodiment reduces the oxygen content of molten steel to 63 ppm after RH decarburization.

[0061] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of the different aspects of the invention as described above exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.

Claims

1. A method for reducing the oxygen content of molten steel, characterized in that, include: During the converter smelting stage, the oxygen content of the molten steel is controlled within a predetermined range during tapping based on the carbon-oxygen product of the molten steel at the end of the converter process. During the RH decarburization stage, when the initial oxygen content of the molten steel entering the RH station is greater than the initial carbon content, carbonaceous substances are added to the molten steel for deoxidation. The control of the oxygen content of the molten steel within a predetermined range during tapping based on the carbon-oxygen product at the converter endpoint includes: When the carbon-oxygen product of the molten steel at the end of the converter is less than or equal to 0.0020%·%, the oxygen content of the molten steel during tapping should be controlled at 350–450 ppm; when the carbon-oxygen product of the molten steel at the end of the converter is greater than 0.0020%·% and less than or equal to 0.0025%·%, the oxygen content of the molten steel during tapping should be controlled at 450–550 ppm; when the carbon-oxygen product of the molten steel at the end of the converter is greater than 0.0025%·%, the oxygen content of the molten steel during tapping should be controlled at 550–650 ppm. When the oxygen content of the molten steel exceeds the upper limit of the predetermined range at the end of the converter, a recarburizing agent is added during the tapping process to deoxidize the steel, so that the oxygen content of the molten steel is within the predetermined range during the tapping process; when the oxygen content of the molten steel is within the predetermined range at the end of the converter, no recarburizing agent is added during the tapping process.

2. The method according to claim 1, characterized in that, During the RH decarburization stage, natural decarburization is carried out when the initial oxygen content of the molten steel entering the RH station is less than the initial carbon content.

3. The method according to claim 1, characterized in that, The carbon-containing substance is added 1.5 to 2 minutes after the RH treatment begins.

4. The method according to claim 1, characterized in that, The carbon-containing material includes carbon-manganese alloys and carbon raisers.

5. The method according to claim 4, characterized in that, The carbon-containing manganese alloy is added all at once, and the carbon raiser is added in batches at intervals.

Citation Information

Patent Citations

  • Deoxygenation method

    CN106893800A

  • Method for smelting ultra-low carbon steel by low oxygen site in whole process

    CN109082496A

  • Control method for content of oxygen in molten steel RH vacuum refining furnace

    CN111705178A

  • Ultra-low carbon steel top slag modification process

    CN116287566A