A high-strength grey cast iron and its production process and application
By controlling the weight percentage of Co and Mo and introducing the incubation treatment of silicon carbide and boron nitride ceramic particles, the problem of low tensile strength of gray cast iron is solved, the tensile strength and wear resistance of castings are improved, and the market is satisfied with the high market Requirements of intensity.
Patent Information
- Application Number
- CN202311530680.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-11-16
AI Technical Summary
The tensile strength of gray cast iron is low, which causes the processed castings to crack and cannot meet the market's demand for high strength.
By controlling the sum of the weight percentages of Co and Mo in gray cast iron within the range of 0.5% to 0.6%, silicon carbide and boron nitride ceramic particles are introduced for incubation treatment, and the components and process parameters are adjusted, such as temperature and casting conditions are optimized to optimize gray cast iron. organizational structure.
The tensile strength of gray cast iron is significantly improved, the coarseness of graphite sheets is avoided, and the wear resistance and shock absorption of castings are enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cast iron, and in particular to high-strength grey cast iron and a production process and application thereof. Background Art
[0002] Gray cast iron is a type of cast iron with flake graphite. It is widely used in automobiles, engineering machinery, etc. due to its excellent shock absorption, low notch sensitivity and high wear resistance. However, there are relatively coarse graphite flakes in the gray cast iron structure, and stress concentration is very likely to occur at the tip of the graphite, which leads to low tensile strength and easy cracking and failure of castings made of gray cast iron. With the development of production, the market has put forward higher requirements for the tensile strength of gray cast iron. Therefore, it is of great significance to develop a high-strength gray cast iron. Summary of the invention
[0003] The invention provides a high-strength grey cast iron and a production process and application thereof, which solves the problem of low tensile strength of grey cast iron in the related art.
[0004] The technical solution of the present invention is as follows:
[0005] The invention provides a high-strength gray cast iron, which is composed of the following components in weight percentage: C 3.70%-3.85%, Si 1.30%-1.50%, Mn 0.50%-0.80%, Co 0.25%-0.45%, Mo 0.15%-0.25%, Cu 1.00%-1.40%, B 0.05%-0.10%, N 0.01%-0.03%, P ≤0.08%, S ≤0.06%, and the rest is Fe and other inevitable impurities;
[0006] The sum of the weight percentages of Co and Mo is 0.5%≤Co+Mo≤0.6%.
[0007] As a further technical solution, the sum of the weight percentages of Co and Mo is 0.55%.
[0008] When the sum of the weight percentages of Co and Mo is 0.55%, the gray cast iron has better tensile strength.
[0009] The present invention also provides a production process of high-strength gray cast iron, comprising the following steps:
[0010] S1. Smelting: weighing various raw materials according to various components of gray cast iron, smelting, and obtaining molten iron;
[0011] S2, inoculation treatment: pouring ceramic particles and inoculant into the molten iron, inoculating, adjusting the composition, and obtaining inoculated molten iron;
[0012] S3, casting: casting the molten iron after inoculation to obtain gray cast iron;
[0013] The ceramic particles include silicon carbide and boron nitride.
[0014] As a further technical solution, the mass ratio of the ceramic particles to the molten iron is 4~6:10000.
[0015] As a further technical solution, the mass ratio of silicon carbide to boron nitride is 1~2:1.
[0016] When the mass ratio of silicon carbide to boron nitride is 1~2:1, the tensile strength of gray cast iron can be further improved.
[0017] As a further technical solution, the particle sizes of the silicon carbide and boron nitride are independently 44-53 μm.
[0018] As a further technical solution, the inoculant is one of ferrosilicon inoculant, silicon-barium inoculant and silicon-strontium inoculant.
[0019] As a further technical solution, the mass ratio of the inoculant to the molten iron is 2~3:1000.
[0020] As a further technical solution, after the smelting, the molten iron is kept at 1530-1540° C. for 10-20 minutes.
[0021] As a further technical solution, during the inoculation treatment, the temperature is 1400-1500°C.
[0022] As a further technical solution, during the casting, the temperature is 1370-1380°C.
[0023] The invention also proposes the application of the high-strength grey cast iron in automobile cast iron products.
[0024] The working principle and beneficial effects of the present invention are:
[0025] 1. In the present invention, by controlling the sum of the weight percentages of Co and Mo in the gray cast iron within the range of 0.5% to 0.6%, pearlite refinement can be effectively promoted and the tensile strength of the gray cast iron can be enhanced. When the sum of the weight percentages of Co and Mo is less than 0.5%, the pearlite refinement effect is not obvious; when the sum of the weight percentages of Co and Mo is greater than 0.6%, the gray cast iron segregates severely, resulting in a decrease in tensile strength.
[0026] 2. In the present invention, by introducing silicon carbide and boron nitride into the gray cast iron structure, on the one hand, the second phase precipitation strengthening effect is achieved, and on the other hand, the wetting angle of graphite is reduced, more heterogeneous nucleation points are provided for graphite, the nucleation rate of graphite is increased, thereby reducing the size of graphite and further improving the tensile strength of gray cast iron. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A production process of high-strength grey cast iron comprises the following steps:
[0030] S1. Smelting: according to the target composition of gray cast iron, scrap iron (Fe 91.5wt%), ferromanganese (Mn 81.3wt%), pure cobalt, ferromolybdenum (Mo 57.6wt%), pure copper, ferrosilicon (Si 83.5wt%), and ferroboron (B 16.4wt%) are weighed and smelted to obtain molten iron;
[0031] S2, inoculation treatment: after the molten iron is kept at 1530°C for 20 minutes, 75SiFe inoculant is poured into the molten iron, and inoculated at 1400°C to adjust the composition and obtain the inoculated molten iron;
[0032] Among them, the mass ratio of 75SiFe inoculant to molten iron is 2:1000;
[0033] S3, casting: casting the inoculated molten iron at 1370° C. to obtain gray cast iron;
[0034] Gray cast iron is composed of the following components in weight percentage: C 3.72%, Si 1.33%, Mn 0.51%, Co 0.26%, Mo 0.24%, Cu 1.03%, B 0.05%, N 0.01%, P 0.07%, S 0.05%, and the rest is Fe and other inevitable impurities.
[0035] Example 2
[0036] A production process of high-strength grey cast iron comprises the following steps:
[0037] S1. Smelting: according to the target composition of gray cast iron, scrap iron (Fe 91.5wt%), ferromanganese (Mn 81.3wt%), pure cobalt, ferromolybdenum (Mo 57.6wt%), pure copper, ferrosilicon (Si 83.5wt%), and ferroboron (B 16.4wt%) are weighed and smelted to obtain molten iron;
[0038] S2, inoculation treatment: after the molten iron is kept at 1540°C for 10 minutes, 75SiFe inoculant is poured into the molten iron, and inoculation treatment is performed at 1500°C to adjust the composition to obtain the inoculated molten iron;
[0039] Among them, the mass ratio of 75SiFe inoculant to molten iron is 3:1000;
[0040] S3, casting: casting the inoculated molten iron at 1380° C. to obtain gray cast iron;
[0041] Gray cast iron is composed of the following components in weight percentage: C 3.84%, Si 1.48%, Mn 0.79%, Co 0.45%, Mo 0.15%, Cu 1.38%, B 0.10%, N 0.03%, P 0.06%, S 0.05%, and the rest is Fe and other inevitable impurities.
[0042] Example 3
[0043] The only difference between this embodiment and embodiment 2 is that, in this embodiment, the gray cast iron is composed of the following components in weight percentage: C 3.84%, Si 1.48%, Mn 0.79%, Co 0.25%, Mo 0.25%, Cu 1.38%, B 0.10%, N 0.03%, P 0.06%, S 0.05%, and the rest is Fe and other inevitable impurities, and the addition amount of raw materials such as scrap iron, ferromanganese, pure cobalt, ferromolybdenum, pure copper, ferrosilicon, and ferroboron is adjusted according to this target component.
[0044] Example 4
[0045] The only difference between this embodiment and embodiment 2 is that, in this embodiment, the gray cast iron is composed of the following components in weight percentage: C 3.84%, Si 1.48%, Mn 0.79%, Co 0.30%, Mo 0.25%, Cu 1.38%, B 0.10%, N 0.03%, P 0.06%, S 0.05%, and the rest is Fe and other inevitable impurities, and the addition amount of raw materials such as scrap iron, ferromanganese, pure cobalt, ferromolybdenum, pure copper, ferrosilicon, and ferroboron is adjusted according to this target component.
[0046] Example 5
[0047] The difference between this embodiment and embodiment 4 is that, in this embodiment, silicon carbide ceramic particles (with a particle size of 44 μm) are also flushed into the molten iron during the inoculation process;
[0048] Among them, the mass ratio of silicon carbide ceramic particles to molten iron is 5:10000;
[0049] After inoculation, the composition is adjusted so that the gray cast iron consists of the following components in weight percentage: C 3.84%, Si 1.48%, Mn 0.79%, Co 0.30%, Mo 0.25%, Cu 1.38%, B 0.10%, N 0.03%, P 0.06%, S 0.05%, and the rest is Fe and other inevitable impurities.
[0050] Example 6
[0051] The only difference between this embodiment and embodiment 5 is that in this embodiment, the ceramic particles are boron nitride (particle size is 44 μm).
[0052] Example 7
[0053] The only difference between this embodiment and embodiment 5 is that in this embodiment, the ceramic particles are composed of silicon carbide (particle size is 44 μm) and boron nitride (particle size is 44 μm) in a mass ratio of 1:2.
[0054] Example 8
[0055] The only difference between this embodiment and embodiment 5 is that in this embodiment, the ceramic particles are composed of silicon carbide (particle size is 44 μm) and boron nitride (particle size is 44 μm) in a mass ratio of 3:1.
[0056] Example 9
[0057] The only difference between this embodiment and embodiment 5 is that in this embodiment, the ceramic particles are composed of silicon carbide (particle size is 44 μm) and boron nitride (particle size is 44 μm) in a mass ratio of 1:1.
[0058] Example 10
[0059] The only difference between this embodiment and embodiment 5 is that in this embodiment, the ceramic particles are composed of silicon carbide (particle size is 44 μm) and boron nitride (particle size is 44 μm) in a mass ratio of 2:1.
[0060] Comparative Example 1
[0061] The only difference between this comparative example and Example 1 is that, in this comparative example, the gray cast iron is composed of the following components in weight percentage: C 3.72%, Si 1.33%, Mn 0.51%, Co 0.26%, Mo 0.15%, Cu 1.03%, B 0.05%, N 0.01%, P 0.07%, S 0.05%, and the rest is Fe and other inevitable impurities, and the addition amount of raw materials such as scrap iron, ferromanganese, pure cobalt, ferromolybdenum, pure copper, ferrosilicon, and ferroboron is adjusted according to this target component.
[0062] Comparative Example 2
[0063] The only difference between this comparative example and Example 1 is that, in this comparative example, the gray cast iron is composed of the following components in weight percentage: C 3.72%, Si 1.33%, Mn 0.51%, Co 0.45%, Mo 0.25%, Cu 1.03%, B 0.05%, N 0.01%, P0.07%, S 0.05%, and the rest is Fe and other inevitable impurities, and the addition amount of raw materials such as scrap iron, ferromanganese, pure cobalt, ferromolybdenum, pure copper, ferrosilicon, and ferroboron is adjusted according to this target component.
[0064] The tensile strength of the gray cast iron produced in Examples 1 to 10 and Comparative Examples 1 to 2 was tested according to GB / T 9439-2023 "Gray Cast Iron Parts", wherein the specimens were type A specimens. The test results are shown in Table 1 below.
[0065] Table 1 Tensile strength test results
[0066]
[0067] Comparison between Example 1 and Comparative Examples 1-2 shows that when the sum of the weight percentages of Co and Mo is in the range of 0.5%-0.6%, the gray cast iron has a higher tensile strength. Comparison between Example 4 and Examples 2-3 shows that when the sum of the weight percentages of Co and Mo is 0.55%, the gray cast iron has a better tensile strength. Comparison between Example 4 and Examples 5-10 shows that by introducing ceramic particles into the gray cast iron structure, the tensile strength of the gray cast iron can be further improved. Comparison between Examples 5-6 and Examples 7-10 shows that when the ceramic particles are composed of silicon carbide and boron nitride, the tensile strength of the gray cast iron can be further improved. Comparison between Examples 7-8 and Examples 9-10 shows that when the mass ratio of silicon carbide to boron nitride is 1-2:1, the tensile strength of the gray cast iron can be further improved.
[0068] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength grey cast iron, characterized in that: It is composed of the following components in weight percentage: C 3.70%~3.85%, Si1.30%~1.50%, Mn 0.50%~0.80%, Co 0.25%~0.45%, Mo 0.15%~0.25%, Cu 1.00%~1.40%, B0.05%~0.10%, N 0.01%~0.03%, P≤0.08%, S≤0.06%, and the rest is Fe and other inevitable impurities; The sum of the weight percentages of Co and Mo is 0.5%≤Co+Mo≤0.6%; The production process of the grey cast iron comprises the following steps: S1. Smelting: weighing various raw materials according to various components of gray cast iron, smelting, and obtaining molten iron; S2, inoculation treatment: pouring ceramic particles and inoculant into the molten iron, inoculating, adjusting the composition, and obtaining inoculated molten iron; S3, casting: casting the molten iron after inoculation to obtain gray cast iron; The ceramic particles include silicon carbide and boron nitride; The particle sizes of the silicon carbide and boron nitride are independently 44-53 μm; The mass ratio of silicon carbide to boron nitride is 1-2:
1.
2. The high-strength gray cast iron according to claim 1, characterized in that: The sum of the weight percentages of Co and Mo is 0.55%.
3. A production process for high-strength grey cast iron, characterized in that: The following steps are involved: S1. Smelting: weighing raw materials for each component of the high-strength gray cast iron according to any one of claims 1 to 2, and smelting to obtain molten iron; S2, inoculation treatment: pouring ceramic particles and inoculant into the molten iron, inoculating, adjusting the composition, and obtaining inoculated molten iron; S3, casting: casting the molten iron after inoculation to obtain gray cast iron; The ceramic particles include silicon carbide and boron nitride.
4. A production process for high-strength grey cast iron according to claim 3, characterized in that: The mass ratio of silicon carbide to boron nitride is 1-2:
1.
5. The production process of high-strength grey cast iron according to claim 3, characterized in that: The particle sizes of the silicon carbide and the boron nitride are independently 44-53 μm.
6. The production process of high-strength grey cast iron according to claim 3, characterized in that: The inoculant is one of ferrosilicon inoculant, silicon-barium inoculant and silicon-strontium inoculant.
7. The production process of high-strength grey cast iron according to claim 3, characterized in that: After the smelting, the molten iron is kept at 1530-1540° C. for 10-20 minutes.
8. The production process of high-strength grey cast iron according to claim 3, characterized in that: During the inoculation treatment, the temperature is 1400-1500°C.
9. The production process of high-strength grey cast iron according to claim 3, characterized in that: During the casting, the temperature is 1370-1380°C.
10. Use of the high-strength grey cast iron according to any one of claims 1 to 2 or the high-strength grey cast iron produced according to the production process of high-strength grey cast iron according to any one of claims 3 to 9 in automotive cast iron products.