Aramid honeycomb core base paper, method for preparing aramid honeycomb core paper, and aramid honeycomb

By applying glue and step-by-step drying and curing on the aramid honeycomb core base paper, combined with step-by-step hot pressing treatment, the problem of insufficient strength of low-quantitative aramid honeycomb paper in the high-end field is solved, and the overall strength and preparation efficiency of the paper are improved. Meets application needs in aerospace and other fields.

CN117513064BActive Publication Date: 2024-11-26SHANDONG RENFENG SPECIAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311698940.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2024-11-26
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

The medium and low quantitative aramid honeycomb paper in the prior art is difficult to meet the strength needs of high-end fields such as aerospace, rail transit, and ships, resulting in less application in these fields.

Method used

By applying glue on the surface of the aramid honeycomb core base paper, UV photocuring resin with a molecular weight greater than or equal to 5000 is used, and step-by-step drying and curing treatment is carried out, combined with step-by-step hot pressing treatment to enhance the connection between fibers and the overall paper. strength.

Benefits of technology

It improves the strength and preparation efficiency of aramid honeycomb core paper, avoids local shrinkage and damage of paper, and meets the mechanical and structural performance requirements of high-end fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117513064B_ABST
    Figure CN117513064B_ABST
Patent Text Reader

Abstract

The present disclosure provides an aramid honeycomb core paper, a method for preparing the aramid honeycomb core paper, and an aramid honeycomb, which relates to the field of honeycomb paper technology, and solves the problem of poor strength of existing aramid honeycombs. The method for preparing the aramid honeycomb core paper comprises: performing a molding process on a mixed pulp containing aramid fibers and precipitated fibers to obtain a molding paper; performing a sizing process on the surface of the molding paper; performing a dehydration process on the molding paper after the sizing process to obtain a dehydrated paper; and performing a drying and curing process on the dehydrated paper to obtain an aramid honeycomb core paper. The method for preparing the aramid honeycomb core paper provided in the present disclosure is used to prepare aramid honeycomb core paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of honeycomb paper, and in particular to an aramid honeycomb core base paper, a preparation method of the aramid honeycomb core paper, and an aramid honeycomb. Background Art

[0002] As a high-strength material, aramid honeycomb has a wide range of application prospects. However, there are few low-weight aramid honeycombs that meet the use requirements of high-end fields such as aviation, rail transportation, and ships. Summary of the invention

[0003] The purpose of the present disclosure is to provide an aramid honeycomb core base paper and a method for preparing the aramid honeycomb core paper and an aramid honeycomb, which are used to prepare the aramid honeycomb core base paper, the aramid honeycomb core paper and the aramid honeycomb with high strength.

[0004] In order to achieve the above objectives, the present disclosure provides the following technical solutions:

[0005] A method for preparing aramid honeycomb core base paper, the method comprising:

[0006] Performing molding treatment on the mixed pulp containing aramid fibers and precipitated fibrids to obtain a molded base paper;

[0007] Performing sizing treatment on the surface of the molding base paper, wherein the sizing treatment glue solution comprises a UV light-curable resin having a molecular weight greater than or equal to 5000;

[0008] Dehydrating the formed base paper after the sizing treatment to obtain dehydrated base paper;

[0009] The dehydrated base paper is subjected to a drying and curing treatment to obtain an aramid honeycomb core base paper, wherein the drying temperature in the drying and curing treatment is increased in a step-by-step manner.

[0010] Compared with the prior art, in the preparation method of the aramid honeycomb core base paper provided by the present invention, by applying glue on the surface of the molded base paper, the glue solution is fully infiltrated into the fiber gaps of the molded base paper, so that the connection between the fibers is tighter, and the loss of fibers during the dehydration process is reduced. At the same time, since the glue solution selected by the present invention includes a UV light-curing resin with a molecular weight greater than or equal to 5000, the high molecular weight UV light-curing resin has a high molecular cross-linking degree after ultraviolet light irradiation, when the dehydrated base paper containing the glue solution of the resin is irradiated with ultraviolet light, the UV light-curing resin is cured, so that the combination between the fibers of the shaped base paper is tighter, and the overall strength of the paper is improved. In addition, since the UV light-curing resin has a fast curing speed when irradiated with ultraviolet light, the preparation efficiency of the aramid honeycomb core base paper is relatively high. Based on this, when the dehydrated base paper containing the glue solution is dried and cured, since the drying temperature during the drying and curing treatment is stepped up, it can further avoid the situation where the water or other solvents in the dehydrated base paper are rapidly volatilized due to direct high-temperature drying treatment, resulting in local shrinkage and damage of the paper, and avoid the occurrence of paper diseases.

[0011] The present disclosure also provides an aramid honeycomb core base paper, wherein the aramid honeycomb core base paper is prepared by the above-mentioned method for preparing the aramid honeycomb core base paper.

[0012] Compared with the prior art, the beneficial effects of the aramid honeycomb core base paper provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here.

[0013] The present disclosure also provides a method for preparing an aramid honeycomb core paper, the method comprising: subjecting the aramid honeycomb core paper to a step-by-step hot pressing treatment to obtain the aramid honeycomb core paper, wherein the temperatures of two adjacent steps in the step-by-step hot pressing treatment are increased in a step-by-step manner.

[0014] Compared with the prior art, the beneficial effects of the method for preparing the aramid honeycomb core paper provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here.

[0015] The present disclosure also provides an aramid honeycomb core paper, which is prepared by the above-mentioned method for preparing the aramid honeycomb core base paper.

[0016] Compared with the prior art, the beneficial effects of the aramid honeycomb core paper provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here.

[0017] The present disclosure also provides an aramid honeycomb, comprising the above-mentioned aramid honeycomb base paper.

[0018] Compared with the prior art, the beneficial effects of the aramid honeycomb provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings described herein are used to provide a further understanding of the present disclosure and constitute a part of the present disclosure. The illustrative embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure. In the drawings:

[0020] Figure 1 A flow chart showing a method for preparing an aramid honeycomb core base paper according to an exemplary embodiment of the present disclosure is shown;

[0021] Figure 2 A flow chart of a method for preparing a mixed pulp containing aramid fibers and fibrids provided according to an exemplary embodiment of the present disclosure is shown;

[0022] Figure 3 A flow chart of dehydrating the formed base paper after sizing treatment according to an exemplary embodiment of the present disclosure is shown;

[0023] Figure 4 A flow chart of performing step-by-step hot pressing treatment on the aramid honeycomb core base paper according to an exemplary embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0024] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.

[0025] Various structural schematic diagrams according to embodiments of the present disclosure are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may further design regions / layers with different shapes, sizes, and relative positions according to actual needs.

[0026] In the context of the present disclosure, when a layer / element is referred to as being "on" another layer / element, the layer / element may be directly on the other layer / element, or there may be an intermediate layer / element between them. In addition, if a layer / element is "on" another layer / element in one orientation, then when the orientation is reversed, the layer / element may be "under" the other layer / element. In order to make the technical problems, technical solutions and beneficial effects to be solved by the present disclosure clearer, the present disclosure is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not intended to limit the present disclosure.

[0027] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present disclosure, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.

[0028] In the description of the present disclosure, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.

[0029] With the increasing demand for high-strength materials, aramid honeycomb, as a high-strength material, has broad application prospects. High strength refers to the ability of a material to maintain high strength and stiffness when subjected to external forces, which has important engineering significance. Aramid honeycomb materials have the advantages of light weight, high strength, and corrosion resistance. Lightweight materials bring many advantages to the development of aerospace and high-speed rail, such as reducing aircraft costs, improving fuel efficiency, and increasing load capacity. They can be widely used in aerospace, automobiles, ships and other fields.

[0030] However, judging from the current market application of products, low-weight aramid honeycomb paper is rarely used in high-end fields such as aerospace, rail transportation, and ships. Therefore, it is urgent to improve the strength of aramid honeycomb materials to further expand its application areas and improve product performance, so that the mechanical and structural properties of meta-aramid honeycomb paper can meet the application of high-end fields such as aerospace, rail transportation, and ships. It should be understood that the low weight here can be aramid honeycomb paper with a weight of 10 g / m2 ~30g / m 2 .

[0031] In order to overcome the above problems, the present disclosure provides an aramid honeycomb core paper, a method for preparing the aramid honeycomb core paper, and an aramid honeycomb. The aramid honeycomb core paper prepared by the method for preparing the aramid honeycomb core paper disclosed in the present disclosure has high strength, so that the aramid honeycomb prepared by the aramid honeycomb core paper has high strength, which can meet the application needs of high-end fields such as aerospace, rail transportation, and ships.

[0032] Figure 1 FIG. 1 is a flow chart showing a method for preparing an aramid honeycomb core base paper according to an exemplary embodiment of the present disclosure. Figure 1 As shown, the method for preparing the aramid honeycomb core base paper provided by the exemplary embodiment of the present disclosure includes:

[0033] Step 110: forming the mixed pulp containing aramid fibers and precipitated fibers to obtain formed base paper.

[0034] The aramid fiber involved in the exemplary embodiment of the present disclosure may be aramid short fibers, which may be meta-aramid short fibers, para-aramid short fibers, or mixed fibers of meta-aramid short fibers and para-aramid short fibers, etc., but are not limited thereto. The length of the aramid fiber may be 3 mm to 8 mm, and the diameter of the aramid fiber may be 5 μm to 10 μm. For example, the length of the aramid fiber may be 3 mm, 5 mm, 7 mm, or 8 mm, etc., but are not limited thereto. The diameter of the aramid fiber may be 5 μm, 7 μm, 8 μm, or 10 μm, etc., but are not limited thereto.

[0035] In order to further increase the strength of the aramid honeycomb core base paper, a high modulus fiber with a modulus greater than 200CN / dkex may be added to the raw material of the aramid honeycomb core base paper provided by the exemplary embodiment of the present disclosure. The high modulus fiber may include one or more of carbon fiber, poly(p-phenylene benzobisoxazole) fiber, basalt fiber, and polymer polyethylene fiber. For example, the high modulus fiber may be carbon fiber, poly(p-phenylene benzobisoxazole) fiber, basalt fiber, polymer polyethylene fiber, or carbon fiber, poly(p-phenylene benzobisoxazole) fiber, basalt fiber, and polymer polyethylene fiber.

[0036] The fibrids involved in the exemplary embodiments of the present disclosure may include one or more of aramid fibrids, arylsulfone fibrids and polyimide fibrids. For example, the fibrids may be aramid fibrids, arylsulfone fibrids, polyimide fibrids, aramid fibrids, arylsulfone fibrids and polyimide fibrids, etc., but are not limited thereto. Among them, the aramid fibrids may include one or a combination of two of meta-aramid fibrids and para-aramid fibrids. For example, the aramid fibrids may be meta-aramid fibrids, para-aramid fibrids, meta-aramid fibrids and para-aramid fibrids, etc., but are not limited thereto.

[0037] Step 120: Sizing is performed on the surface of the molding base paper, and the glue solution of the sizing treatment includes a UV light-curable resin with a molecular weight greater than or equal to 5000. By performing the sizing treatment on the surface of the molding base paper, the glue solution can fully penetrate into the fibers of the molding base paper, thereby ensuring that the fibers can be tightly bonded together in subsequent processes such as dehydration, thereby avoiding the occurrence of powder loss.

[0038] When the raw materials provided by the exemplary embodiment of the present disclosure include high modulus fibers, the high modulus fibers, aramid fibers and precipitated fibers can be tightly connected together through sizing treatment, ensuring that the evenly dispersed fiber structure after slurry mixing will not be destroyed in subsequent processing steps, thereby improving the overall performance of the finished product.

[0039] Step 130: Dehydrate the sizing treated formed base paper to obtain dehydrated base paper. It should be understood that the wet papermaking process provided by the exemplary embodiment of the present disclosure is a conventional process, and the equipment used is also commonly used equipment in the art, which will not be explained separately in the present disclosure.

[0040] Step 140: Drying and curing the dehydrated base paper to obtain aramid honeycomb core base paper, wherein the drying temperature in the drying and curing process is increased in a step-by-step manner. Through the drying and curing process, and the drying temperature in the drying and curing process is increased in a step-by-step manner, the phenomenon of local shrinkage and damage of the paper caused by the rapid volatilization of water and other solvents in the glue solution can be avoided, thereby avoiding the occurrence of paper diseases.

[0041] In summary, in the preparation method of the aramid honeycomb core base paper provided by the present disclosure, by applying glue on the surface of the molded base paper, the glue solution is fully infiltrated into the fiber gaps of the molded base paper, so that the connection between the fibers is closer, and the loss of fibers during the dehydration process is reduced. At the same time, since the glue solution selected by the present disclosure includes a UV light-curing resin with a molecular weight greater than or equal to 5000, the use of the UV light-curing resin as the main component of the glue solution can avoid the problem of local shrinkage and damage of the paper due to the volatilization of water and other solvents in the glue solution before the drying process. And the high molecular weight UV light-curing resin has a high molecular cross-linking degree after ultraviolet light irradiation. When the dehydrated base paper containing the glue solution of the resin is irradiated with ultraviolet light, the UV light-curing resin is cured, so that the bonding between the fibers of the shaped base paper is closer, and the overall strength of the paper is improved. In addition, since the UV light-curing resin has a fast curing speed when irradiated with ultraviolet light, the preparation efficiency of the aramid honeycomb core base paper is relatively high. Based on this, when the dehydrated base paper containing glue is dried and solidified, since the drying temperature during the drying and solidification treatment is increased in a step-by-step manner, it can further avoid the situation where the water or other solvents in the dehydrated base paper evaporate rapidly due to direct high-temperature drying treatment, causing local shrinkage and damage of the paper, and avoid the occurrence of paper diseases.

[0042] As a possible implementation, Figure 2 FIG. 1 is a flow chart showing a method for preparing a mixed pulp containing aramid fibers and fibrids according to an exemplary embodiment of the present disclosure. Figure 2 As shown, before the mixed pulp containing aramid fibers and fibrids is subjected to the molding process, the method provided by the exemplary embodiment of the present disclosure further includes:

[0043] Step 210: The aramid fibers are dispersed to obtain aramid fiber slurry. The concentration of the aramid fiber slurry is 0.05‰~1‰. For example, the concentration of the aramid fiber slurry can be 0.05‰, 0.07‰, 0.2‰, 0.5‰, 0.7‰, 1‰, etc., but not limited thereto. The time for the dispersion can be 5min~8min, so that the aramid fibers can be fully dispersed. For example, the time can be 5min, 7min, 8min, etc., but not limited thereto.

[0044] In practical applications, when the aramid fiber is dispersed, the functional additives can be used to achieve the desired dispersion effect of the aramid fiber. It should be understood that the functional additives here may include: one or more of a retention agent, a defoamer, a dispersant and a hydrophilic agent, and the selection of the additives can be determined according to actual conditions. For example, the functional additives may include a retention agent, a defoamer, a dispersant, a hydrophilic agent, a retention agent, a defoamer, a dispersant and a hydrophilic agent, etc., but are not limited thereto.

[0045] The retention aid may include cationic starch and / or polyethyleneimine. For example, the retention aid may include cationic starch, may include polyethyleneimine, or may include cationic starch and polyethyleneimine.

[0046] The defoamer may include a polysiloxane defoamer and / or a polyether-modified silicone oil. For example, the defoamer may include a polysiloxane defoamer, may include a polyether-modified silicone oil, or may include a polysiloxane defoamer and a polyether-modified silicone oil.

[0047] The hydrophilic agent may include polyvinyl alcohol and / or polyacrylic acid. For example, the hydrophilic agent may include polyvinyl alcohol, may include polyacrylic acid, or may include polyvinyl alcohol and polyacrylic acid.

[0048] The above-mentioned dispersant may include polyethylene oxide and / or cationic polyacrylamide. For example, the dispersant may include polyethylene oxide, may include cationic polyacrylamide, and may also include polyethylene oxide and cationic polyacrylamide.

[0049] Step 220: Beat and disperse the fibrid to obtain a fibrid slurry. The beating degree of the fibrid can be 25°SR to 80°SR. For example, the beating degree of the fibrid can be 25°SR, 55°SR, 75°SR, or 80°SR, etc., but is not limited thereto. The beating concentration of the fibrid slurry can be 0.5% to 1%. For example, the beating concentration of the fibrid slurry can be 0.5%, 0.7%, or 1%, etc., but is not limited thereto.

[0050] Step 230: Mix the aramid fiber slurry and the fibrillation slurry to obtain a mixed slurry containing aramid fibers and fibrillation. The mass ratio of the aramid fibers to the fibrillation may be (1:4) to (4:1). For example, the mass ratio of the aramid fibers to the fibrillation may be 1:4, 2:1, or 4:1, etc., but is not limited thereto. The mixing and decomposition time may be 8 minutes to 12 minutes to ensure that the mixed fibers can be fully decomposed and evenly dispersed. For example, the time may be 8 minutes, 10 minutes, or 12 minutes, etc., but is not limited thereto.

[0051] As a possible implementation, the solid content of the UV light-curable resin is 30% to 45% of the mass of the glue solution. For example, the solid content of the UV light-curable resin can be 30% of the mass of the glue solution, can be 40% of the mass of the glue solution, or can be 45% of the mass of the glue solution. The UV light-curable resin can include one or more of polyurethane acrylate, epoxy acrylate, polyester acrylate resin, and amino acrylate resin. For example, the UV light-curable resin can include polyurethane acrylate, epoxy acrylate, polyester acrylate resin, amino acrylate resin, polyurethane acrylate, epoxy acrylate, polyester acrylate resin, and amino acrylate resin, etc., but is not limited thereto. By using a glue solution with a solid content that meets the above requirements, the amount of glue applied to the paper web during the coating operation of the equipment is within a reasonable range, which is beneficial to improving the strength of the paper, and avoiding the difficulty of drying the wet paper web and the difficulty of light curing the glue solution due to the high amount of glue, which reduces the preparation efficiency, reduces the paper void structure, and is not conducive to the subsequent preparation of aramid honeycomb impregnation with resin.

[0052] As a possible implementation, the glue solution of the sizing treatment also includes a photoinitiator, which accounts for 0.1% to 3% of the solid content of the UV light-curing resin. For example, the photoinitiator can account for 0.1% of the solid content of the UV light-curing resin, can account for 0.3% of the solid content of the UV light-curing resin, and can also account for 3% of the solid content of the UV light-curing resin. The photoinitiator can include 2-hydroxy-2-methyl-1-phenylacetone and / or 1-hydroxycyclohexyl phenyl ketone. For example, the photoinitiator can include 2-hydroxy-2-methyl-1-phenylacetone, can include 1-hydroxycyclohexyl phenyl ketone, and can also include 2-hydroxy-2-methyl-1-phenylacetone and 1-hydroxycyclohexyl phenyl ketone. It should be understood that the main function of the photoinitiator here is to initiate a cross-linking reaction between unsaturated resin molecules, so that the light-curing resin can be cured more firmly. Therefore, by using a photoinitiator that meets the above requirements, it is possible to avoid the problem that too little photoinitiator addition will not cause the unsaturated bonds of polymer and monomer molecules to generate free radicals, and that free radical chain polymerization reactions will be carried out in a short time to crosslink and form a network structure macromolecule. At the same time, it is possible to avoid the problem that too much photoinitiator addition may cause excessive light consumption, thereby reducing the degree of curing, or producing too many by-products, which will affect the quality of the finished paper.

[0053] As a possible implementation method, the amount of the glue applied is 1% to 10% of the absolute dry fiber mass of the mixed pulp. This allows the glue to fully penetrate into the fibers of the shaped base paper, exerting the effects of bonding and increasing strength, while avoiding the problem that the paper is too hard, easily damaged, and difficult to roll up due to the excessive content of UV light-curing resin in the final product. The amount of glue applied here can be 1% of the absolute dry fiber mass of the mixed pulp, 5% of the absolute dry fiber mass of the mixed pulp, or 10% of the absolute dry fiber mass of the mixed pulp, etc., and is not limited thereto.

[0054] As a possible implementation, Figure 3 FIG. 1 shows a flow chart of dehydrating the formed base paper after sizing treatment according to an exemplary embodiment of the present disclosure. Figure 3 As shown, the dehydration treatment of the formed base paper after the sizing treatment may include:

[0055] Step 310: performing natural gravity dehydration treatment on the sizing-treated formed base paper to obtain pre-dehydrated base paper.

[0056] Step 320: The pre-dehydrated base paper is subjected to vacuum filtration treatment to obtain pre-made base paper, and the vacuum degree of the vacuum filtration treatment is -0.1MPa~-5MPa. For example, the vacuum degree can be -0.1MPa, -0.5MPa, -0.7MPa, -1MPa, -2MPa, -2.5MPa, or -5MPa, etc., and is not limited thereto. By combining natural gravity dehydration and vacuum filtration, the paper sheet forming effect is better and the process complexity is lower. At the same time, since the negative vacuum degree can make the paper easier to decouple, it can be avoided that the wet paper web adsorbs the forming net during natural gravity dehydration or vacuum dehydration, resulting in the phenomenon that the wet paper web is not easy to peel off, thereby causing paper breakage. Based on this, during the vacuum filtration treatment, the air in the vacuum tank can be evacuated by a vacuum pump to form a negative pressure, thereby improving the dehydration efficiency. At the same time, a certain pressure will be generated on the paper under the negative pressure state, so that the flatness of the blank is improved, and the thickness difference of the blank is small, so as to meet the requirements of subsequent processing.

[0057] As a possible implementation method, the above-mentioned drying and curing treatment of the dehydrated base paper may include: first, performing a multi-stage drying treatment on the dehydrated base paper to obtain a dried base paper. Among them, the multi-stage drying treatment includes at least a three-stage drying treatment, and the temperature of the first-stage drying treatment is 30°C~45°C, for example, the temperature can be 30°C, 40°C, or 45°C, etc., but is not limited to this. The temperature of the second-stage drying treatment is 60°C~75°C, for example, the temperature can be 60°C, 70°C, or 75°C, etc., but is not limited to this. The temperature of the third-stage drying treatment is 90°C~105°C, for example, the temperature can be 90°C, 100°C, or 105°C, etc., but is not limited to this. Then, the dried base paper is cured to obtain an aramid honeycomb core base paper. It should be noted that in order to improve the overall performance of the aramid honeycomb core base paper finally obtained, the drying stages of the multi-stage drying treatment can be set to multiple stages, and the specific stages can be selected according to actual conditions, and are not limited here. The multi-stage drying process can avoid the occurrence of blistering and cracking of the glue layer, thereby improving the overall performance of the aramid honeycomb core base paper finally prepared.

[0058] The exemplary embodiment of the present disclosure further provides an aramid honeycomb core base paper, which is prepared by the above-mentioned method for preparing the aramid honeycomb core base paper.

[0059] Compared with the prior art, the beneficial effects of the aramid honeycomb core base paper provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here.

[0060] The exemplary embodiment of the present disclosure also provides a method for preparing aramid honeycomb core paper, the method comprising: performing a step-by-step hot pressing treatment on the aramid honeycomb core base paper to obtain the aramid honeycomb core paper, wherein the temperature of two adjacent steps in the step-by-step hot pressing treatment is increased in a step-by-step manner. By adopting the step-by-step hot pressing treatment, and the temperature of two adjacent steps in the step-by-step hot pressing treatment is increased in a step-by-step manner, the phenomenon of paper shrinkage and cracks caused by different thermal shrinkage rates of fiber raw materials can be effectively reduced, and the density of the prepared aramid honeycomb core paper is high.

[0061] As a possible implementation, Figure 4 FIG. 1 shows a flow chart of performing a step-by-step hot pressing process on the aramid honeycomb core base paper according to an exemplary embodiment of the present disclosure. Figure 4 As shown, the aramid honeycomb core base paper is subjected to a step-by-step hot pressing treatment, which may include:

[0062] Step 410: preheat and press the aramid honeycomb core base paper to obtain preheated base paper. The preheat and press temperature may be 150°C to 180°C, for example, 150°C, 170°C, 180°C, etc., but is not limited thereto.

[0063] Step 420: hard press the preheated base paper to obtain aramid honeycomb core paper, and the temperature of the hard pressing treatment is greater than the temperature of the preheating pressing treatment. The temperature of the hard pressing treatment can be 220°C to 280°C, for example, the temperature can be 220°C, 250°C, or 280°C, etc., but is not limited thereto. The speed of the hard pressing treatment is 5m / min to 40m / min, for example, the speed can be 5m / min, 25m / min, or 40m / min, etc., but is not limited thereto. The pressure of the hard pressing treatment is 1MPa to 30MPa, and the pressure can be 1MPa, 25MPa, or 30MPa, etc., but is not limited thereto.

[0064] In some optional ways, before the preheated base paper is hard pressed, the method further includes: spraying an aqueous solution on the surface of the preheated base paper, the aqueous solution may include water and an anti-sticking agent, the mass of the anti-sticking agent is 0.5% to 20% of the mass of the aqueous solution, for example, the mass of the anti-sticking agent may be 0.5% of the mass of the aqueous solution, 2.5% of the mass of the aqueous solution, 7.5% of the mass of the aqueous solution, 15.5% of the mass of the aqueous solution, or 20% of the mass of the aqueous solution, etc., and is not limited thereto. The coating amount of the aqueous solution is 2% to 5% of the weight of the preheated base paper, for example, the coating amount of the aqueous solution may be 2% of the weight of the preheated base paper, 3% of the weight of the preheated base paper, or 5% of the weight of the preheated base paper, etc., and is not limited thereto. The anti-sticking agent may be a polytetrafluoroethylene emulsion and / or a calcium stearate emulsion, for example, the anti-sticking agent may be a polytetrafluoroethylene emulsion, a calcium stearate emulsion, or a polytetrafluoroethylene emulsion and / or a calcium stearate emulsion. In order to reduce the impact of ions on the comprehensive properties of paper, deionized water can be used. By spraying deionized water containing anti-sticking agent before hard pressing, the paper can be prevented from sticking to the roller during hard pressing, thereby avoiding paper failure, protecting equipment, and avoiding the impact on the paper's quantitative and smoothness. At the same time, the consistency of paper thickness and surface flatness can be improved, and the occurrence of paper powder can be reduced.

[0065] The exemplary embodiment of the present disclosure further provides an aramid honeycomb core paper, which is prepared by the above-mentioned method for preparing the aramid honeycomb core base paper.

[0066] Compared with the prior art, the beneficial effects of the aramid honeycomb core paper provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here.

[0067] The exemplary embodiment of the present disclosure further provides an aramid honeycomb, comprising the above-mentioned aramid honeycomb core paper.

[0068] Compared with the prior art, the beneficial effects of the aramid honeycomb provided in the present disclosure are the same as the beneficial effects of the method for preparing the aramid honeycomb core base paper described in the above technical solution, and will not be described in detail here.

[0069] The present disclosure is further described below by way of examples, but the present disclosure is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product instructions.

[0070] Example 1

[0071] The aramid fiber selected in this embodiment is a meta-aramid short fiber with a length of 3 mm and a diameter of 5 μm, the selected precipitated fiber is a meta-aramid precipitated fiber, the selected UV light-curable resin is polyurethane acrylate, the selected photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, the selected anti-sticking agent is polytetrafluoroethylene emulsion, and the water in the aqueous solution is deionized water.

[0072] (1) Preparation of aramid honeycomb core paper

[0073] The meta-aramid short fibers were dispersed and decomposed in water for 8 minutes to obtain an aramid fiber pulp with a concentration of 0.05‰; the meta-aramid fibrid was beaten to 30°SR to obtain a fibrid pulp with a beating concentration of 0.5%; the aramid fiber pulp and the fibrid pulp were blended in a mass ratio of aramid fiber to fibrid of 4:6 to obtain a mixed pulp containing aramid fiber and fibrid, and the mixing and decomposition time was 10 minutes. Then the mixed pulp containing aramid fiber and fibrid was transported to an inclined wire paper machine for forming to obtain a formed base paper, and the surface of the formed base paper was sizing treated at the end of the forming wire, and the sizing treatment glue liquid included a UV light-curable water-based polyurethane acrylate glue liquid, the solid content of the polyurethane acrylate in the glue liquid was 30%, the sizing amount was 3% of the absolute dry fiber mass of the mixed pulp, and the photoinitiator in the glue liquid accounted for 0.1% of the solid content of the UV light-curable resin. The shaped base paper after the sizing treatment is subjected to natural gravity dehydration treatment and -2Mpa vacuum filtration dehydration treatment to obtain dehydrated base paper. The dehydrated base paper is sent to a three-stage drying oven for three-stage drying treatment to obtain dry base paper; wherein, the temperature of the drying oven for the first stage drying treatment is 30°C, the temperature of the drying oven for the second stage drying treatment is 60°C, and the temperature of the drying oven for the third stage drying treatment is 100°C. The dry base paper passing through the third stage drying oven is sent to the UV light curing area, and after ultraviolet light radiation, the glue is rapidly cured, and after winding, the aramid honeycomb core base paper is obtained.

[0074] (2) Preparation of aramid honeycomb core paper

[0075] The aramid honeycomb core paper is preheated and pressed at 170°C to obtain preheated paper, and an aqueous solution containing an anti-adhesive agent is sprayed on the surface of the preheated paper, wherein the mass of the anti-adhesive agent is 0.5% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 5% of the weight of the preheated paper. Then, the preheated paper sprayed with the aqueous solution is sent into a hard pressing roller for hard pressing to obtain aramid honeycomb core paper. The hard pressing temperature is 220°C, the speed of the hard pressing is 10m / min, and the pressure of the hard pressing is 15MPa. The properties of the prepared aramid honeycomb core paper are shown in Table 1.

[0076] (3) Preparation of aramid honeycomb

[0077] Coat the surface of the aramid honeycomb core paper with core glue strips at equal intervals, then overlap and bond the upper and lower layers of honeycomb core paper with offset core glue strips to form a thick plate, and perform hot pressing and curing to obtain a bonded thick plate, wherein the hot pressing temperature is 100°C, the hot pressing pressure is 0.5MPa, and the hot pressing time is 5min. Immerse the bonded thick plate in phenolic resin glue for 15min, take it out and stretch it along the stacking direction of the bonded thick plate at a stretching speed of 5mm / min, and dry and cure it after stretching to obtain a shaped thick plate, the drying and curing temperature is 120°C, and the drying and curing time is 0.5h. Immerse the shaped thick plate in epoxy resin glue for 20min, then take it out for high-temperature curing to obtain an aramid honeycomb, the curing temperature is 130°C, and the curing time is 0.5h. Finally, cut the aramid honeycomb into pieces according to needs.

[0078] Example 2

[0079] The aramid fiber selected in this embodiment is para-aramid short-cut fiber with a length of 5 mm and a diameter of 7 μm, the selected precipitated fiber is meta-aramid precipitated fiber, the selected UV light-curing resin is polyurethane acrylate, the selected photoinitiator is 1-hydroxycyclohexyl phenyl ketone, the selected anti-sticking agent is calcium stearate emulsion, and the water in the aqueous solution is deionized water.

[0080] (1) Preparation of aramid honeycomb core paper

[0081] The para-aramid short fibers were dispersed and decomposed in water for 5 minutes to obtain an aramid fiber pulp with a concentration of 0.5‰; the meta-aramid fibrid was beaten to 45°SR to obtain a fibrid pulp with a beating concentration of 0.7%; the aramid fiber pulp and the fibrid pulp were blended in a mass ratio of aramid fiber to fibrid of 1:4 to obtain a mixed pulp containing aramid fiber and fibrid, and the mixing and decomposition time was 8 minutes. Then the mixed pulp containing aramid fiber and fibrid was transported to an inclined wire paper machine for forming to obtain a formed base paper, and the surface of the formed base paper was sizing treated at the end of the forming wire, and the sizing treatment glue liquid included a UV light-curable water-based polyurethane acrylate glue liquid, the solid content of the polyurethane acrylate in the glue liquid was 40%, the sizing amount was 5% of the absolute dry fiber mass of the mixed pulp, and the photoinitiator in the glue liquid accounted for 0.5% of the solid content of the UV light-curable resin. The shaped base paper after the sizing treatment is subjected to natural gravity dehydration treatment and -3Mpa vacuum filtration dehydration treatment to obtain dehydrated base paper. The dehydrated base paper is sent to a three-stage drying oven for a three-stage drying treatment to obtain dry base paper; wherein the temperature of the drying oven for the first stage drying treatment is 40°C, the temperature of the drying oven for the second stage drying treatment is 65°C, and the temperature of the drying oven for the third stage drying treatment is 105°C. The dry base paper passing through the third stage drying oven is sent to the UV light curing area, and after ultraviolet light radiation, the glue is rapidly cured, and after winding, the aramid honeycomb core base paper is obtained.

[0082] (2) Preparation of aramid honeycomb core paper

[0083] The aramid honeycomb core paper is preheated and pressed at 150°C to obtain preheated paper, and an aqueous solution containing an anti-adhesive agent is sprayed on the surface of the preheated paper, wherein the mass of the anti-adhesive agent is 1% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 3% of the weight of the preheated paper. Then, the preheated paper sprayed with the aqueous solution is sent into a hard pressing roller for hard pressing to obtain aramid honeycomb core paper. The hard pressing temperature is 240°C, the vehicle speed is 5m / min, and the pressure is 1MPa. The properties of the prepared aramid honeycomb core paper are shown in Table 1.

[0084] (3) Preparation of aramid honeycomb

[0085] The surface of the aramid honeycomb core paper is coated with core glue strips at equal intervals, and then the upper and lower layers of the honeycomb core paper with offset core glue strips are overlapped and bonded into a thick plate, and hot pressing and curing are performed to obtain a bonded thick plate, wherein the hot pressing temperature is 170°C, the hot pressing pressure is 1 MPa, and the hot pressing time is 1min. The bonded thick plate is immersed in phenolic resin glue for 25min, and after being taken out, it is stretched along the stacking direction of the bonded thick plate at a stretching speed of 100mm / min. After the stretching is completed, it is dried and cured to obtain a shaped thick plate, and the drying and curing temperature is 130°C and the drying and curing time is 0.7h. The shaped thick plate is immersed in phenolic resin doped with 8wt% ammonium polyphosphate for 30min, and then taken out for high-temperature curing to obtain an aramid honeycomb, and the curing temperature is 150°C and the curing time is 1h. Finally, the aramid honeycomb can be cut into pieces according to needs.

[0086] Example 3

[0087] The aramid fiber selected in this embodiment is a mixed fiber of meta-aramid short fibers and para-aramid short fibers with a length of 8 mm and a diameter of 10 μm, the selected precipitated fibers are a mixed fiber of para-aramid precipitated fibers and aromatic sulfone precipitated fibers, the selected UV light-curing resin is epoxy acrylate, the selected photoinitiator is 1-hydroxycyclohexyl phenyl ketone, the selected anti-sticking agent is polytetrafluoroethylene emulsion and calcium stearate emulsion, and the water in the aqueous solution is deionized water.

[0088] (1) Preparation of aramid honeycomb core paper

[0089] The aramid fiber was dispersed and decomposed in water for 7 minutes to obtain an aramid fiber pulp with a concentration of 1‰; the fibrillation was beaten to 25°SR to obtain a fibrillation pulp with a beating concentration of 1%; the aramid fiber pulp and the fibrillation pulp were blended in a mass ratio of aramid fiber to fibrillation of 4:1 to obtain a mixed pulp containing aramid fiber and fibrillation, and the mixing and decomposition time was 12 minutes. Then the mixed pulp containing aramid fiber and fibrillation was transported to a slant wire paper machine for forming to obtain a formed base paper, and the surface of the formed base paper was sizing treated at the end of the forming wire. The sizing treatment glue liquid included UV light-curable water-based polyurethane acrylate glue liquid, the solid content of polyurethane acrylate in the glue liquid was 45%, the sizing amount was 1% of the absolute dry fiber mass of the mixed pulp, and the photoinitiator in the glue liquid accounted for 2% of the solid content of the UV light-curable resin. The formed base paper after sizing treatment was subjected to natural gravity dehydration treatment and -0.1Mpa vacuum filtration dehydration treatment to obtain dehydrated base paper. The dehydrated base paper is sent to a three-stage drying oven for three-stage drying treatment to obtain dry base paper; wherein the temperature of the drying oven for the first stage drying treatment is 45°C, the temperature of the drying oven for the second stage drying treatment is 75°C, and the temperature of the drying oven for the third stage drying treatment is 90°C. The dry base paper passing through the third stage drying oven is sent to the UV light curing area, and after ultraviolet light radiation, the glue is quickly cured, and after winding, the aramid honeycomb core base paper is obtained.

[0090] (2) Preparation of aramid honeycomb core paper

[0091] The aramid honeycomb core paper is preheated and pressed at 180°C to obtain preheated paper, and an aqueous solution containing an anti-adhesive agent is sprayed on the surface of the preheated paper, wherein the mass of the anti-adhesive agent is 20% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 2% of the weight of the preheated paper. Then, the preheated paper sprayed with the aqueous solution is sent into a hard pressing roller for hard pressing to obtain aramid honeycomb core paper. The hard pressing temperature is 280°C, the speed of the hard pressing is 40m / min, and the pressure of the hard pressing is 30MPa. The properties of the prepared aramid honeycomb core paper are shown in Table 1.

[0092] (3) Preparation of aramid honeycomb

[0093] The surface of the aramid honeycomb core paper is coated with core glue strips at equal intervals, and then the upper and lower layers of the honeycomb core paper with offset core glue strips are overlapped and bonded into a thick plate, and hot pressing and curing are performed to obtain a bonded thick plate, wherein the hot pressing temperature is 220°C, the hot pressing pressure is 2 MPa, and the hot pressing time is 3min. The bonded thick plate is immersed in phenolic resin glue for 30min, and after being taken out, it is stretched along the stacking direction of the bonded thick plate at a stretching speed of 200mm / min. After the stretching is completed, it is dried and cured to obtain a shaped thick plate, and the drying and curing temperature is 150°C and the drying and curing time is 1h. The shaped thick plate is immersed in phenolic resin with 10wt% aluminum hydroxide for 45min, and then taken out for high-temperature curing to obtain an aramid honeycomb, and the curing temperature is 180°C and the curing time is 1.5h. Finally, the aramid honeycomb can be cut into pieces according to needs.

[0094] Example 4

[0095] The aramid fiber selected in this embodiment is a mixed fiber of meta-aramid short-cut fibers with a length of 8 mm and a diameter of 10 μm, the selected precipitated fibers are polyimide precipitated fibers, the selected UV light-curable resins are polyester acrylic resins and amino acrylic resins, the selected photoinitiators are 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycyclohexyl phenyl ketone, the selected anti-sticking agent is polytetrafluoroethylene emulsion, and the water in the aqueous solution is deionized water.

[0096] (1) Preparation of aramid honeycomb core paper

[0097] The aramid fiber was dispersed and decomposed in water for 7 minutes to obtain an aramid fiber pulp with a concentration of 1‰; the fibrillation was beaten to 80°SR to obtain a fibrillation pulp with a beating concentration of 1%; the aramid fiber pulp and the fibrillation pulp were blended in a mass ratio of aramid fiber to fibrillation of 4:1 to obtain a mixed pulp containing aramid fiber and fibrillation, and the mixing and decomposition time was 12 minutes. Then the mixed pulp containing aramid fiber and fibrillation was transported to an inclined wire paper machine for forming to obtain a formed base paper, and the surface of the formed base paper was sizing treated at the end of the forming wire. The sizing treatment glue liquid included UV light-curing water-based polyurethane acrylate glue liquid, the solid content of polyurethane acrylate in the glue liquid was 45%, the sizing amount was 10% of the absolute dry fiber mass of the mixed pulp, and the photoinitiator in the glue liquid accounted for 3% of the solid content of the UV light-curing resin. The formed base paper after sizing treatment was subjected to natural gravity dehydration treatment and -5Mpa vacuum filtration dehydration treatment to obtain dehydrated base paper. The dehydrated base paper is sent to a three-stage drying oven for three-stage drying treatment to obtain dry base paper; wherein the temperature of the drying oven for the first stage drying treatment is 45°C, the temperature of the drying oven for the second stage drying treatment is 75°C, and the temperature of the drying oven for the third stage drying treatment is 90°C. The dry base paper passing through the third stage drying oven is sent to the UV light curing area, and after ultraviolet light radiation, the glue is quickly cured, and after winding, the aramid honeycomb core base paper is obtained.

[0098] (2) Preparation of aramid honeycomb core paper

[0099] The aramid honeycomb core paper is preheated and pressed at 180°C to obtain preheated paper, and an aqueous solution containing an anti-adhesive agent is sprayed on the surface of the preheated paper, wherein the mass of the anti-adhesive agent is 20% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 2% of the weight of the preheated paper. Then, the preheated paper sprayed with the aqueous solution is sent into a hard pressing roller for hard pressing to obtain aramid honeycomb core paper. The hard pressing temperature is 280°C, the speed of the hard pressing is 40m / min, and the pressure of the hard pressing is 30MPa. The properties of the prepared aramid honeycomb core paper are shown in Table 1.

[0100] (3) Preparation of aramid honeycomb

[0101] The surface of the aramid honeycomb core paper is coated with core glue strips at equal intervals, and then the upper and lower layers of the honeycomb core paper with offset core glue strips are overlapped and bonded into a thick plate, and hot pressing and curing are performed to obtain a bonded thick plate, wherein the hot pressing temperature is 220°C, the hot pressing pressure is 2 MPa, and the hot pressing time is 3min. The bonded thick plate is immersed in phenolic resin glue for 30min, and after being taken out, it is stretched along the stacking direction of the bonded thick plate at a stretching speed of 200mm / min. After the stretching is completed, it is dried and cured to obtain a shaped thick plate, and the drying and curing temperature is 150°C and the drying and curing time is 1h. The shaped thick plate is immersed in phenolic resin with 10wt% aluminum hydroxide for 45min, and then taken out for high-temperature curing to obtain an aramid honeycomb, and the curing temperature is 180°C and the curing time is 1.5h. Finally, the aramid honeycomb can be cut into pieces according to needs.

[0102] Comparative Example 1

[0103] In this embodiment, the aramid fiber selected is meta-aramid short-cut fiber with a length of 3 mm and a diameter of 5 μm, the selected fibrils are meta-aramid fibrils, the selected anti-adhesive agent is polytetrafluoroethylene emulsion, and the water in the aqueous solution is deionized water.

[0104] (1) Preparation of aramid honeycomb core paper

[0105] The meta-aramid short fibers were dispersed and decomposed in water for 8 minutes to obtain an aramid fiber pulp with a concentration of 0.05‰; the meta-aramid fibrid was beaten to 30°SR to obtain a fibrid pulp with a beating concentration of 0.5%; the aramid fiber pulp and the fibrid pulp were blended in a mass ratio of aramid fiber to fibrid of 4:6 to obtain a mixed pulp containing aramid fiber and fibrid, and the mixing and decomposition time was 10 minutes. Then the mixed pulp containing aramid fiber and fibrid was transported to an inclined wire paper machine for forming to obtain a formed base paper. The formed base paper was subjected to natural gravity dehydration treatment and -2Mpa vacuum filtration dehydration treatment to obtain a dehydrated base paper. The dehydrated base paper was sent to a three-stage drying oven for a three-stage drying treatment to obtain a dry base paper; wherein the temperature of the drying oven for the first stage drying treatment was 30°C, the temperature of the drying oven for the second stage drying treatment was 60°C, and the temperature of the drying oven for the third stage drying treatment was 100°C. Finally, after winding, the aramid honeycomb core base paper was obtained.

[0106] (2) Preparation of aramid honeycomb core paper

[0107] The aramid honeycomb core paper is preheated and pressed at 170°C to obtain preheated paper, and an aqueous solution containing an anti-adhesive agent is sprayed on the surface of the preheated paper, wherein the mass of the anti-adhesive agent is 0.5% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 5% of the weight of the preheated paper. Then, the preheated paper sprayed with the aqueous solution is sent into a hard pressing roller for hard pressing to obtain aramid honeycomb core paper. The hard pressing temperature is 220°C, the speed of the hard pressing is 10m / min, and the pressure of the hard pressing is 15MPa. The properties of the prepared aramid honeycomb core paper are shown in Table 1.

[0108] (3) Preparation of aramid honeycomb

[0109] Coat the surface of the aramid honeycomb core paper with core glue strips at equal intervals, then overlap and bond the upper and lower layers of honeycomb core paper with offset core glue strips to form a thick plate, and perform hot pressing and curing to obtain a bonded thick plate, wherein the hot pressing temperature is 100°C, the hot pressing pressure is 0.5MPa, and the hot pressing time is 5min. Immerse the bonded thick plate in phenolic resin glue for 15min, take it out and stretch it along the stacking direction of the bonded thick plate at a stretching speed of 5mm / min, and dry and cure it after stretching to obtain a shaped thick plate, the drying and curing temperature is 120°C, and the drying and curing time is 0.5h. Immerse the shaped thick plate in epoxy resin glue for 20min, then take it out for high-temperature curing to obtain an aramid honeycomb, the curing temperature is 130°C, and the curing time is 0.5h. Finally, cut the aramid honeycomb into pieces according to needs.

[0110] Comparative Example 2

[0111] The aramid fiber selected in this embodiment is a meta-aramid short fiber with a length of 3 mm and a diameter of 5 μm, the selected precipitated fiber is a meta-aramid precipitated fiber, the selected UV light-curable resin is polyurethane acrylate, the selected photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, the selected anti-sticking agent is polytetrafluoroethylene emulsion, and the water in the aqueous solution is deionized water.

[0112] (1) Preparation of aramid honeycomb core paper

[0113] The meta-aramid short fibers were dispersed and decomposed in water for 8 minutes to obtain an aramid fiber pulp with a concentration of 0.05‰; the meta-aramid fibrid was beaten to 30°SR to obtain a fibrid pulp with a beating concentration of 0.5%; the aramid fiber pulp and the fibrid pulp were blended in a mass ratio of aramid fiber to fibrid of 4:6 to obtain a mixed pulp containing aramid fiber and fibrid, and the mixing and decomposition time was 10 minutes. Then the mixed pulp containing aramid fiber and fibrid was transported to an inclined wire paper machine for forming to obtain a formed base paper, and the surface of the formed base paper was sizing treated at the end of the forming wire, and the sizing treatment glue liquid included UV light-curing water-based polyurethane acrylate glue liquid, the solid content of polyurethane acrylate in the glue liquid was 30%, the sizing amount was 3% of the absolute dry fiber mass of the mixed pulp, and the photoinitiator in the glue liquid accounted for 0.1% of the solid content of the UV light-curing resin. The formed base paper after sizing treatment was dehydrated by natural gravity to obtain a dehydrated base paper. The dehydrated base paper is sent to a three-stage drying oven for three-stage drying treatment to obtain dry base paper; wherein the temperature of the drying oven for the first stage drying treatment is 30°C, the temperature of the drying oven for the second stage drying treatment is 60°C, and the temperature of the drying oven for the third stage drying treatment is 100°C. The dry base paper passing through the third stage drying oven is sent to the UV light curing area, and after ultraviolet light radiation, the glue is quickly cured, and after winding, the aramid honeycomb core base paper is obtained.

[0114] (2) Preparation of aramid honeycomb core paper

[0115] The aramid honeycomb core paper is preheated and pressed at 170°C to obtain preheated paper, and an aqueous solution containing an anti-adhesive agent is sprayed on the surface of the preheated paper, wherein the mass of the anti-adhesive agent is 0.5% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 4% of the weight of the preheated paper. Then, the preheated paper sprayed with the aqueous solution is sent into a hard pressing roller for hard pressing to obtain aramid honeycomb core paper. The hard pressing temperature is 220°C, the speed of the hard pressing is 13m / min, and the pressure of the hard pressing is 15MPa. The properties of the prepared aramid honeycomb core paper are shown in Table 1.

[0116] (3) Preparation of aramid honeycomb

[0117] Coat the surface of the aramid honeycomb core paper with core glue strips at equal intervals, then overlap and bond the upper and lower layers of honeycomb core paper with offset core glue strips to form a thick plate, and perform hot pressing and curing to obtain a bonded thick plate, wherein the hot pressing temperature is 100°C, the hot pressing pressure is 0.5MPa, and the hot pressing time is 5min. Immerse the bonded thick plate in phenolic resin glue for 15min, take it out and stretch it along the stacking direction of the bonded thick plate at a stretching speed of 5mm / min, and dry and cure it after stretching to obtain a shaped thick plate, the drying and curing temperature is 120°C, and the drying and curing time is 0.5h. Immerse the shaped thick plate in epoxy resin glue for 20min, then take it out for high-temperature curing to obtain an aramid honeycomb, the curing temperature is 130°C, and the curing time is 0.5h. Finally, cut the aramid honeycomb into pieces according to needs.

[0118] Table 1 Performance of aramid honeycomb core paper

[0119]

[0120] By comparing Examples 1 to 4 in Table 1 with Comparative Example 1, it can be seen that the tensile strength and the difference in smoothness on both sides of the aramid honeycomb core paper prepared by Examples 1 to 4 of the present disclosure are significantly higher than those of Comparative Example 1, and the air permeability is significantly lower than that of Comparative Example 1. It can be seen that the aramid honeycomb core paper prepared by the method disclosed in the present disclosure has higher strength and stronger comprehensive performance after sizing treatment. By comparing Examples 1 to 4 in Table 1 with Comparative Example 2, it can be seen that the tensile strength, elongation and air permeability of the aramid honeycomb core paper prepared by Examples 1 to 4 of the present disclosure are not much different from those of the aramid honeycomb core paper prepared by Comparative Example 2, but the difference in smoothness on both sides is significantly greater than that of Comparative Example 2. It can be seen that the method disclosed in the present disclosure combines natural gravity dehydration treatment and vacuum water filtration treatment to make the prepared aramid honeycomb core paper have a higher paper flatness, which can improve the overall performance of the aramid honeycomb core paper.

[0121] In the above description, the technical details of the patterning and etching of each layer are not described in detail. However, those skilled in the art should understand that various technical means can be used to form layers, regions, etc. of desired shapes. In addition, in order to form the same structure, those skilled in the art can also design methods that are not completely the same as the methods described above. In addition, although the various embodiments are described above separately, this does not mean that the measures in the various embodiments cannot be used in combination to advantage.

[0122] The embodiments of the present disclosure are described above. However, these embodiments are for illustrative purposes only and are not intended to limit the scope of the present disclosure. The scope of the present disclosure is defined by the appended claims and their equivalents. Without departing from the scope of the present disclosure, a person skilled in the art may make a variety of substitutions and modifications, which should all fall within the scope of the present disclosure.

Claims

1. A method for preparing aramid honeycomb core base paper, characterized in that: The method comprises: The aramid fibers are dispersed to obtain aramid fiber slurry; Beating and dispersing the fibrides to obtain a fibrides slurry; The aramid fiber slurry and the fibrid slurry are mixed to obtain a mixed slurry containing aramid fiber and fibrid; the mass ratio of the aramid fiber to the fibrid is (1:4) to (4:1); the concentration of the aramid fiber slurry is 0.05‰ to 1‰; Performing a molding process on the mixed pulp containing aramid fibers and precipitated fibrids to obtain a molded base paper; Performing sizing treatment on the surface of the molding base paper, wherein the sizing treatment glue solution comprises a UV light-curable resin having a molecular weight greater than or equal to 5000; Performing natural gravity dehydration on the sizing-treated formed base paper to obtain pre-dehydrated base paper; The pre-dehydrated base paper is subjected to vacuum filtration treatment to obtain dehydrated base paper, wherein the vacuum degree of the vacuum filtration treatment is -0.1MPa to -5MPa; Performing a multi-stage drying treatment on the dehydrated base paper to obtain a dried base paper, wherein the multi-stage drying treatment includes at least three-stage drying treatments, the temperature of the first-stage drying treatment is 30° C. to 45° C., the temperature of the second-stage drying treatment is 60° C. to 75° C., and the temperature of the third-stage drying treatment is 90° C. to 105° C.; The dried base paper is cured to obtain aramid honeycomb core base paper; the solid content of the UV light-curing resin is 30% to 45% of the mass of the glue solution; the UV light-curing resin includes one or more of polyurethane acrylate, epoxy acrylate, polyester acrylic resin and amino acrylic resin; the glue solution for sizing treatment also includes a photoinitiator, and the photoinitiator accounts for 0.1% to 3% of the solid content of the UV light-curing resin; the sizing amount of the glue solution is 1% to 10% of the absolute dry fiber mass of the mixed pulp.

2. A kind of aramid honeycomb core base paper, characterized in that: The aramid honeycomb core base paper is prepared by the preparation method of the aramid honeycomb core base paper according to claim 1.

3. A method for preparing aramid honeycomb core paper, characterized in that: The method comprises: performing step-by-step hot pressing treatment on the aramid honeycomb core base paper of claim 2 to obtain the aramid honeycomb core paper, wherein the temperatures of two adjacent steps in the step-by-step hot pressing treatment are increased in a step-by-step manner.

4. The method according to claim 3, characterized in that The stepwise hot pressing treatment of the aramid honeycomb core base paper of claim 2 comprises: Preheating and pressing the aramid honeycomb core base paper to obtain preheated base paper; The preheated base paper is subjected to a hard pressing treatment to obtain an aramid honeycomb core paper, wherein the temperature of the hard pressing treatment is greater than the temperature of the preheat pressing treatment.

5. The method according to claim 4, characterized in that The temperature of the preheating and pressing treatment is 150°C to 180°C, the temperature of the hard pressing treatment is 220°C to 280°C, the vehicle speed of the hard pressing treatment is 5m / min to 40m / min, and the pressure of the hard pressing treatment is 1MPa to 30MPa; and / or, Before the hard pressing treatment is performed on the preheated base paper, the method further comprises: An aqueous solution is sprayed on the surface of the preheated base paper, wherein the aqueous solution includes water and a release agent, the mass of the release agent is 0.5% to 20% of the mass of the aqueous solution, and the coating amount of the aqueous solution is 2% to 5% of the weight of the preheated base paper.

6. A kind of aramid honeycomb core paper, characterized in that: The aramid honeycomb core paper is prepared by the preparation method of the aramid honeycomb core base paper according to any one of claims 3 to 5.

7. An aramid honeycomb, characterized in that: Comprising the aramid honeycomb core paper as described in claim 6.