Preparation method of double-anti-release PET support film for OLED

By preparing a dual-resistant release PET support film, the multi-layer antistatic structure is formed by using oxidized nanocellulose and lignocellulose, the deformation and insufficient antistatic properties of the flexible OLED substrate are solved, and the friction resistance of the device is improved. Antistatic properties extend service life.

CN117535020BActive Publication Date: 2024-11-19AZUSA TECH (SHENZHEN) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311397622.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2024-11-19
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

The substrate of flexible OLED devices is thin and easy to deform, which affects its user experience and life. It is necessary to introduce a support film to improve stiffness and friction resistance, and the antistatic performance of the support film is insufficient.

Method used

Using the preparation method of the dual-anti-anti-release PET support film, the oxidized nanocellulose and lignocellulose are prepared to form a four-layer dual-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti-anti Enhance its bonding strength and anti-static properties.

Benefits of technology

The high friction resistance and anti-static properties of the PET support film are achieved, which extends the service life of OLED devices and improves the stiffness of the flexible OLED substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535020B_ABST
    Figure CN117535020B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a double-anti-release PET support film for OLED, which specifically comprises the following steps: step 1, preparing oxidized nanocellulose; step 2, preparing wood cellulose; step 3, preparing an antistatic coating I according to the oxidized nanocellulose prepared in step 1, and preparing an adhesive according to the wood cellulose prepared in step 2; step 4, preparing a double-anti-release PET support film according to the antistatic coating II and the antistatic coating I and the adhesive prepared in step 3. The PET support film prepared by the invention has good antistatic performance and friction resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer composite materials and relates to a method for preparing a double-anti-release PET support film for OLED. Background Art

[0002] OLED (organic light-emitting diode) is widely used in the display and lighting fields. As a new display technology, OLED is favored by more and more people. With the development of OLED display technology, the screen size has changed from small to large. The biggest feature of flexible OLED devices is that the substrate is very thin and flexible, which makes the device insufficiently stiff and easy to deform, greatly affecting the user experience and service life of flexible OLED. Therefore, it is necessary to introduce a support film into the flexible OLED substrate to improve its stiffness and reduce deformation. The better the friction resistance and antistatic properties of the support film, the longer the service life of the OLED device can be. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a double-anti-release PET support film for OLED. The PET support film prepared by the method has good antistatic performance and friction resistance.

[0004] The technical solution adopted by the present invention is a method for preparing a double-anti-release PET support film for OLED, which specifically comprises the following steps:

[0005] Step 1, preparing oxidized nanocellulose;

[0006] Step 2, preparing lignocellulose;

[0007] Step 3, preparing an antistatic coating I according to the oxidized nanocellulose prepared in step 1, and preparing an adhesive according to the wood cellulose prepared in step 2;

[0008] Step 4, preparing a double-anti-release PET support film according to the antistatic coating II and the antistatic coating I prepared in step 3 and the adhesive.

[0009] The present invention is also characterized in that:

[0010] The specific process of step 1 is:

[0011] Step 1.1, taking 2g-3g of cotton fiber with a beating degree of 90, adding 0.1g-0.2g of cellulose complex enzyme and stirring at 35℃-50℃ for 3h~5h to pre-treat the fiber, inactivating it for 10min-15min after the reaction, filtering it and washing it with 100mL-200mL of deionized water, repeating 6~8 times to obtain pre-treated fiber;

[0012] Step 1.2, adding 1000 mL-1500 mL of deionized water to the pretreated fiber obtained in step 1.1 and ultrasonically dispersing it, then adding 0.02 mol / g-0.03 mol / g of 2,2,6,6-tetramethylpiperidine nitrogen oxide and 0.4 mol / g-0.6 mol / g of NaBr, and then adding NaOH to adjust the pH of the reaction system to alkaline, and then adding 100 mL-150 mL of NaClO solution dropwise to the alkaline solution, continuing to stir for 3h-5h, and after the reaction is completed, adding hydrochloric acid to adjust the pH to neutral to obtain a suspension;

[0013] Step 1.3, filter the suspension prepared in step 1.2, wash with 500 mL-1000 mL of deionized water, repeat 6-8 times, and freeze-dry at -70°C to -40°C to obtain white powdery oxidized nanocellulose.

[0014] The specific process of step 2 is:

[0015] Step 2.1, adding 0.1g-0.2g of cellulose complex enzyme to brown cellulose, and stirring at 35℃-50℃ for 3h~5h, inactivating in a sterilizing pot for 10-15min after the reaction, filtering and washing with 100-200mL of deionized water, repeating 6-8 times to obtain pretreated brown cellulose;

[0016] Step 2.2, homogenizing the pretreated brown cellulose obtained in step 2.1 for 60-80 times to obtain wood cellulose.

[0017] In step 3, the preparation process of antistatic coating I is:

[0018] The following components are weighed respectively by mass percentage: 2wt%-5wt% of oxidized nanocellulose, 10wt%-15wt% of aqueous polyurethane, 2wt%-5wt% of cationic starch, 0.1wt%-3wt% of isocyanate, 0.002wt%-0.3wt% of wetting agent, and the remaining component is water, and the sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an antistatic coating I is obtained;

[0019] The preparation process of the adhesive is:

[0020] The following components are weighed respectively by mass percentage: 5wt%-10wt% of polyurethane, 5wt%-10wt% of polyvinyl alcohol, 5wt%-10wt% of silicon phosphate, 5wt%-10wt% of acrylate, 5wt%-10wt% of dimethyldivinylsilane, 5wt%-10wt% of epoxy acrylate, 10wt%-20wt% of acrylic acid, 5wt%-10wt% of N-dodecyldimethylamine, and 20wt%-30wt% of cellulose. The sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an adhesive is obtained.

[0021] The specific process of step 4 is:

[0022] Step 4.1, take a PET film with a thickness of 60 um-90 um, and spin-coat a layer of 3um-5um antistatic coating I on the upper surface and the lower surface of the PET film respectively; then dry it at 80℃-120℃ to obtain a double-antistatic substrate for standby use;

[0023] Step 4.2, take a PET film with a thickness of 20um-40um, spin-coat a layer of 3um-5um antistatic coating II on the upper surface and the lower surface of the PET film respectively, and then dry it at 80℃-120℃ to obtain a double anti-release film for standby use;

[0024] Step 4.3, spin-coat a layer of adhesive on the lower surface of the double-anti-resistance substrate prepared in step 4.1 to form a bonding layer with a thickness of 13um-16um, and dry it at 80℃-120℃. Compound the double-anti-resistance substrate with the double-anti-resistance release film prepared in step 4.2 through the bonding layer, roll it up, and mature it at 40°C~50°C for 40h~60h to obtain a double-anti-resistance release PET support film.

[0025] The preparation process of antistatic coating II is:

[0026] The following components are weighed respectively by mass percentage: 10wt%-15wt% waterborne polyurethane, 2wt%-5wt% cationic starch, 0.1wt%-3wt% isocyanate, 0.002wt%-0.3wt% wetting agent, and the remaining component is water. The sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, the antistatic coating II is obtained.

[0027] The beneficial effect of the present invention is that the PET support film prepared by the present invention has four layers of antistatic components in the double-anti-base and double-anti-release film, and the oxidized nanocellulose particles have good friction resistance, and the addition of wood fiber in the binder can achieve fiber reinforcement and form cross-links with polyurethane to improve the bonding strength of the adhesive. The double-anti-base and double-anti-release film structure contain four antistatic layers, which can achieve antistatic effects before and after use. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a comparison chart of the release film peeling force and the adhesion to glass of the double-anti-release PET support film prepared in Example 1 and Comparative Examples 1 to 3 in the preparation method of the double-anti-release PET support film for OLED of the present invention;

[0029] Figure 2 It is a schematic diagram of using the double-anti-release PET support film prepared in the method for preparing the double-anti-release PET support film for OLED of the present invention for flexible OLED.

[0030] In the figure, 1. double-resistance base, 2. adhesive layer, 3. flexible OLED substrate. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] The method for preparing a double-anti-release PET (PET, polyethylene terephthalate) support film for OLED of the present invention specifically comprises the following steps:

[0033] Step 1, preparation of oxidized nanocellulose, the specific process is:

[0034] Take 2g-3g of cotton fiber with a beating degree of 90, add 0.1g-0.2g of cellulose complex enzyme and stir at 35℃-50℃ for 3h~5h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 10min-15min, filter it under reduced pressure and wash it with 100mL-200mL deionized water, repeat 6~8 times to obtain pre-treated fiber. Then add 1000mL-1500mL deionized water to the pre-treated fiber and disperse it ultrasonically. Then add 0.02mol / g-0.03mol / g of 2,2,6,6-tetramethylpiperidinium nitrogen oxide and 0.4mol / g-0.6mol / g of NaBr, then add NaOH to adjust the pH of the reaction system to 10, then add 100mL-150mL of NaClO (0.5mol / g-0.75mol / g) solution dropwise (30min dropwise addition), and continue stirring for 3-5 hours. After the reaction is completed, the temperature is lowered and hydrochloric acid is added to adjust the pH to neutral to obtain a suspension. The suspension is filtered and washed with 500-1000 mL of deionized water, and the process is repeated 6 to 8 times. The suspension is freeze-dried at -70°C to -40°C to obtain white powdery oxidized nanocellulose.

[0035] Step 2, preparation of lignocellulose, the specific process is:

[0036] Take 2g of brown cellulose, add 0.1-0.2g of cellulose complex enzyme and stir at 35℃-50℃ for 3h~5h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 10-15 min, filter under reduced pressure and wash with 100-200mL of deionized water, repeat 6~8 times to obtain pre-treated brown cellulose. Further, use a high-pressure homogenizer to homogenize 60-80 times to obtain wood cellulose.

[0037] Step 3, preparation of double-anti-release PET support film, the specific process is as follows:

[0038] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 60-90 um, and spin-coat a layer of 3-5 um antistatic coating I on the upper and lower surfaces of the PET respectively; then dry it at 80-120℃ for later use.

[0039] Preparation of double anti-release film: First, take a PET film with a thickness of 20-40 um, spin-coat a layer of 3-5 um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 80-120℃ for later use.

[0040] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 13-16 um and dried at 80-120°C, then compounded with the double-anti-release film, rolled up, and aged at 40-50°C for 40-60h to obtain the double-anti-release PET support film.

[0041] Antistatic coating I: 2-5wt% oxidized nanocellulose, 10-15wt% waterborne polyurethane, 2-5wt% cationic starch, 0.1-3wt% isocyanate, 0.002-0.3wt% wetting agent, and the remaining components are water, and the mixture is stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0042] Antistatic coating II: The following components are weighed respectively by mass percentage: 10wt%-15wt% waterborne polyurethane, 2wt%-5wt% cationic starch, 0.1wt%-3wt% isocyanate, 0.002wt%-0.3wt% wetting agent, and the rest is water. The sum of the mass percentages of the above components is 100%, and the mixture is stirred at 600 r / min for 20 min in a mixer.

[0043] The adhesive composition of the bonding layer: polyurethane 5wt%-10wt%, polyvinyl alcohol 5wt%-10wt%, silicon phosphate 5wt%-10wt%, acrylate 5wt%-10wt%, dimethyl divinyl silane 5wt%-10wt%, epoxy acrylate 5wt%-10wt%, acrylic acid 10wt%-20wt%, N-dodecyl dimethylamine 5wt%-10wt%, and wood cellulose 20wt%-30wt%.

[0044] Example 1

[0045] Step 1, preparation of oxidized nanocellulose, the specific process is:

[0046] Take 2g of cotton fiber with a beating degree of 90, add 0.1g of cellulose complex enzyme and stir at 35℃ for 3h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 10min, filter it under reduced pressure and wash it with 100mL of deionized water, repeat 6 times to obtain pre-treated fiber. Then add 1000mL of deionized water to the pre-treated fiber and disperse it ultrasonically. Then add 0.02mol / g of 2,2,6,6-tetramethylpiperidinium nitrogen oxide and 0.4mol / g of NaBr, then add NaOH to adjust the pH of the reaction system to 10, then 100mL of NaClO (0.5 mol / g) solution dropwise (30 min to add), and continue stirring for 3h. After the reaction is completed, cool down and add hydrochloric acid to adjust the pH to neutral to obtain a suspension. After the suspension is filtered and washed with 500mL of deionized water, repeat 6 times, freeze-dry at -70℃ to obtain white powdery oxidized nanocellulose.

[0047] Step 2, preparation of lignocellulose, the specific process is:

[0048] Take 2g of brown cellulose, add 0.1g of cellulose complex enzyme and stir at 35℃ for 3h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 10 min, filter it under reduced pressure and wash it with 100mL of deionized water, repeat 6 times to obtain pre-treated brown cellulose. Further, use a high-pressure homogenizer to homogenize 60 times to obtain wood cellulose.

[0049] Step 3, preparation of double-anti-release PET support film, the structure of the double-anti-release PET support film is 3 layers, the specific process is:

[0050] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 60 um, and spin-coat a layer of 3 um antistatic coating I on the upper and lower surfaces of the PET respectively; then dry it at 80°C for later use.

[0051] Antistatic coating I: 2wt% of oxidized nanocellulose, 10wt% of waterborne polyurethane, 2wt% of cationic starch, 0.1wt% of isocyanate, 0.002wt% of wetting agent and 85.898wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0052] Preparation of double anti-release film: First, take a PET film with a thickness of 20 um, spin-coat a layer of 3 um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 80°C for use.

[0053] Antistatic coating II: 10wt% of waterborne polyurethane, 2wt% of cationic starch, 0.1wt% of isocyanate, 0.002wt% of wetting agent and 87.898wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the coating.

[0054] The adhesive composition of the bonding layer is as follows: 10wt% polyurethane, 10wt% polyvinyl alcohol, 5wt% silicon phosphate, 5wt% acrylate, 5wt% dimethyldivinylsilane, 10wt% epoxy acrylate, 20wt% acrylic acid, 10wt% N-dodecyldimethylamine, and 25%wt wood cellulose.

[0055] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 13 um and dried at 80°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 40°C for 40 hours to obtain the double-anti-release PET support film.

[0056] Comparative Example 1 (Oxidized nanocellulose is removed from antistatic coating 1, and the rest remains unchanged)

[0057] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 60 um, spin-coat a layer of 3 um antistatic coating I on the upper and lower surfaces of the PET, and then dry it at 80°C for use.

[0058] Preparation of double anti-release film: First, take a PET film with a thickness of 20um, spin-coat a layer of 3um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 80℃ for use.

[0059] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 13 um and dried at 80°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 40°C for 40 hours to obtain the double-anti-release PET support film.

[0060] Antistatic coating I: 10 wt% of waterborne polyurethane, 2 wt% of cationic starch, 0.1 wt% of isocyanate, 0.002 wt% of wetting agent, and 87.898 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0061] Antistatic coating II: 10wt% of waterborne polyurethane, 2wt% of cationic starch, 0.1wt% of isocyanate, 0.002wt% of wetting agent and 87.898wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the coating.

[0062] The adhesive composition of the bonding layer is as follows: 10wt% polyurethane, 10wt% polyvinyl alcohol, 5wt% silicon phosphate, 5wt% acrylate, 5wt% dimethyldivinylsilane, 10wt% epoxy acrylate, 20wt% acrylic acid, 10wt% N-dodecyldimethylamine, and 25%wt wood cellulose.

[0063] Comparative Example 2 (removing wood cellulose from the adhesive, and keeping the rest unchanged)

[0064] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 60 um, spin-coat a layer of 3 um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 80°C for use.

[0065] Preparation of double anti-release film: First, take a PET film with a thickness of 20um, spin-coat a layer of 3um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 80℃ for use.

[0066] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 13 um and dried at 80°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 40°C for 40 hours to obtain the double-anti-release PET support film.

[0067] Antistatic coating I: 2% oxidized nanocellulose, 10wt% waterborne polyurethane, 2wt% cationic starch, 0.1wt% isocyanate, 0.002wt% wetting agent, and 85.898wt% water were mixed and stirred in a mixer at 600 r / min for 20 min to obtain the antistatic coating.

[0068] Antistatic coating II: 10 wt% of waterborne polyurethane, 2 wt% of cationic starch, 0.1 wt% of isocyanate, 0.002 wt% of wetting agent, and 87.898 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0069] The adhesive composition of the bonding layer is as follows: 13.3 wt % of polyurethane, 13.3 wt % of polyvinyl alcohol, 6.7 wt % of silicon phosphate, 6.7 wt % of acrylate, 6.7 wt % of dimethyldivinylsilane, 13.3 wt % of epoxy acrylate, 26.7 wt % of acrylic acid, and 13.3 wt % of N-dodecyldimethylamine.

[0070] Comparative Example 3 (removing the antistatic layer I, that is, only a layer of antistatic coating I is spin-coated on the lower surface of the PET film, and the rest remains unchanged)

[0071] Preparation of monoclonal antibody substrate: First, take a PET film with a thickness of 60 um, spin-coat a layer of 3 um antistatic coating I on the lower surface of the PET, and then dry it at 80°C for use.

[0072] Preparation of double anti-release film: First, take a PET film with a thickness of 20um, spin-coat a layer of 3um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 80℃ for use.

[0073] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 13 um and dried at 80°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 40°C for 40 hours to obtain the double-anti-release PET support film.

[0074] Antistatic coating I: 2wt% of oxidized nanocellulose, 10wt% of waterborne polyurethane, 2wt% of cationic starch, 0.1wt% of isocyanate, 0.002wt% of wetting agent and 85.898wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0075] Antistatic coating II: 10 wt% of waterborne polyurethane, 2 wt% of cationic starch, 0.1 wt% of isocyanate, 0.002 wt% of wetting agent, and 87.898 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer.

[0076] The adhesive composition of the bonding layer is as follows: 10wt% polyurethane, 10wt% polyvinyl alcohol, 5wt% silicon phosphate, 5wt% acrylate, 5wt% dimethyldivinylsilane, 10%wt epoxy acrylate, 20wt% acrylic acid, 10wt% N-dodecyldimethylamine, and 25wt% wood cellulose.

[0077] Results and Discussion

[0078] The peeling force of the release film and the adhesion to glass in the product of Example 1 reached 0.07 N / 50mm and 17.5N / 25mm respectively. The mechanical performance requirements of "light peeling and heavy adhesion" of the double-resistant release PET support film were met. However, the binder component in Comparative Example 2 lacked lignocellulose, which lost the mechanical reinforcement and cross-linking effect of lignocellulose, so its adhesion to glass was greatly reduced to 9.8 N / 25mm.

[0079] In Example 1, the introduction of oxidized nanocellulose can improve the friction resistance hardness of the substrate to 3A, while in Comparative Example 1, the wear resistance hardness is only 2A after the lack of oxidized nanocellulose. At the same time, the lack of oxidized nanocellulose in Comparative Example 1 reduces its antistatic property, and the resistance increases from 10 6Reduce by 10 8 ;

[0080] The double-anti-release PET support film used for OLED requires that both the base and the release layer have good antistatic properties, so that the support film is effective during pasting and subsequent use.

[0081] In comparative example 3, after removing the first antistatic layer, the friction hardness of the substrate was reduced to 2A, and the antistatic property was lost, and the resistance was directly increased to 10 12 , the antistatic effect cannot be achieved.

[0082] Figure 1 The figure is a comparison of the release film peeling force and the adhesion to glass of the double-resistant release PET support film in Example 1 and Comparative Examples 1 to 3. The release peeling force of Example 1 and Comparative Examples 1 and 3 is 0.07 N / 50mm; and the adhesion to glass is 17.5 N / 25mm; Comparative Example 2 lacks the mechanical reinforcement and cross-linking effect of wood cellulose, and its release peeling force is reduced to 0.05 N / 50mm, and the adhesion to glass is reduced to 9.8 N / 25mm. The performance tests of Example 1 of the present invention and Comparative Examples 1 to 3 are shown in Table 1 below:

[0083] Table 1. Performance test of double-anti-release PET support film

[0084]

[0085] The double-resistance release PET support film prepared in Example 1 of the present invention is used for flexible OLED. Since the price of flexible substrate raw materials for OLED is high, in order to reduce costs, the thickness of the substrate is reduced as much as possible, usually to about 30um. The thin film thickness will lead to the shortcomings of poor stiffness and easy deformation of flexible OLED. After the double-resistance release layer of the prepared double-resistance release PET support film (size 7x3.8cm) is peeled off, the obtained double-resistance base (thickness 88um) is directly pasted on the surface of the flexible OLED polyimide substrate (size 7x3.8cm, substrate thickness 30um), as shown in FIG. Figure 2 As shown, Figure 2 In the figure, 1 is a double-resistance substrate, 2 is an adhesive layer, and 3 is a flexible OLED substrate.

[0086] The stiffness determination method refers to GB / T10739 standard, and the stiffness of flexible OLED substrate polyimide and double anti-release PET support film are tested. The results show that under the same conditions, the stiffness of flexible OLED substrate polyimide is 26mN; while the stiffness of double anti-release PET support film is 113 mN. The main reason is that after the double anti-release PET support film is attached, the thickness of the flexible OLED substrate is increased from the original 30 um to 118 um.

[0087] Example 2

[0088] Step 1, preparation of oxidized nanocellulose, the specific process is:

[0089] Take 2.5g of cotton fiber with a beating degree of 90, add 0.15g of cellulose complex enzyme and stir at 45℃ for 4h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 12min, filter it under reduced pressure and wash it with 150mL of deionized water, repeat 7 times to obtain pretreated fiber. Then add 1200mL of deionized water to the pretreated fiber and disperse it ultrasonically. Then add 0.025mol / g of 2,2,6,6-tetramethylpiperidinium nitrogen oxide and 0.5mol / g of NaBr, then add NaOH to adjust the pH of the reaction system to 10, then add 120mL of NaClO (0.6 mol / g) solution dropwise (30 min to complete), and continue stirring for 4h. After the reaction is completed, cool it down and add hydrochloric acid to adjust the pH to neutral to obtain a suspension. After the suspension is filtered and washed with 800mL of deionized water, repeat 7 times, and freeze-dry at -50℃ to obtain white powdery oxidized nanocellulose.

[0090] Step 2, preparation of lignocellulose, the specific process is:

[0091] Take 2g of brown cellulose, add 0.15g of cellulose complex enzyme and stir at 45℃ for 4h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 12 min, filter it under reduced pressure and wash it with 150mL of deionized water, repeat 7 times to obtain pre-treated brown cellulose. Then, use a high-pressure homogenizer to homogenize it 70 times to obtain wood cellulose.

[0092] Step 3, preparation of double-anti-release PET support film, the specific process is as follows:

[0093] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 70 um, and spin-coat a layer of 4 um antistatic coating I on the upper and lower surfaces of the PET respectively; then dry it at 100°C for later use.

[0094] Antistatic coating I: 3wt% of oxidized nanocellulose, 12wt% of waterborne polyurethane, 3wt% of cationic starch, 1wt% of isocyanate, 0.2wt% of wetting agent and 80.8wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0095] Preparation of double anti-release film: First, take a PET film with a thickness of 30 um, spin-coat a layer of 4 um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 100°C for use.

[0096] Antistatic coating II: 12 wt% of waterborne polyurethane, 3 wt% of cationic starch, 1 wt% of isocyanate, 0.2 wt% of wetting agent and 83.8 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0097] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 15 um and dried at 100°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 45°C for 50 hours to obtain the double-anti-release PET support film.

[0098] The adhesive composition of the bonding layer is as follows: 5wt% polyurethane, 5wt% polyvinyl alcohol, 10wt% silicon phosphate, 10wt% acrylate, 10wt% dimethyldivinylsilane, 5wt% epoxy acrylate, 17wt% acrylic acid, 8wt% N-dodecyldimethylamine, and 30%wt wood cellulose.

[0099] Example 3

[0100] Step 1, preparation of oxidized nanocellulose, the specific process is:

[0101] Take 3g of cotton fiber with a beating degree of 90, add 0.2g of cellulose complex enzyme and stir at 50℃ for 5h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 15min, filter it under reduced pressure and wash it with 200mL of deionized water, repeat 8 times to obtain pretreated fiber. Then add 1500mL of deionized water to the pretreated fiber and disperse it ultrasonically. Then add 0.03mol / g of 2,2,6,6-tetramethylpiperidinium nitrogen oxide and 0.6mol / g of NaBr, then add NaOH to adjust the pH of the reaction system to 10, then 150mL of NaClO (0.75 mol / g) solution dropwise (30 min to add), and continue stirring for 5h. After the reaction is completed, cool down and add hydrochloric acid to adjust the pH to neutral to obtain a suspension. After the suspension is filtered and washed with 1000mL of deionized water, repeat 8 times, and freeze-dry at -40℃ to obtain white powdery oxidized nanocellulose.

[0102] Step 2, preparation of lignocellulose, the specific process is:

[0103] Take 2g of brown cellulose, add 0.2g of cellulose complex enzyme and stir at 50℃ for 5h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 15 min, filter it under reduced pressure and wash it with 200mL of deionized water, repeat 8 times to obtain pre-treated brown cellulose. Further, use a high-pressure homogenizer to homogenize 80 times to obtain wood cellulose.

[0104] Step 3, preparation of double-anti-release PET support film, the specific process is as follows:

[0105] Preparation of double-antistatic substrate: First, take a 90 um thick PET film, and spin-coat a 5 um layer of antistatic coating I on the upper and lower surfaces of the PET respectively; then dry it at 120°C for later use.

[0106] Antistatic coating I: 5wt% of oxidized nanocellulose, 15wt% of waterborne polyurethane, 5wt% of cationic starch, 3wt% of isocyanate, 0.3wt% of wetting agent and 71.7wt% of water were mixed and stirred in a mixer at 600 r / min for 20 min to obtain the antistatic coating.

[0107] Preparation of double anti-release film: First, take a PET film with a thickness of 30 um, spin-coat a layer of 4 um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 100°C for use.

[0108] Antistatic coating II: 15wt% of waterborne polyurethane, 5wt% of cationic starch, 3wt% of isocyanate, 0.3wt% of wetting agent and 76.7wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0109] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 16 um and dried at 120°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 50°C for 60 hours to obtain the double-anti-release PET support film.

[0110] The adhesive composition of the bonding layer is as follows: 9wt% polyurethane, 9wt% polyvinyl alcohol, 9wt% silicon phosphate, 9wt% acrylate, 9wt% dimethyldivinylsilane, 10wt% epoxy acrylate, 10wt% acrylic acid, 5wt% N-dodecyldimethylamine, and 30%wt wood cellulose.

[0111] Example 4

[0112] Step 1, preparation of oxidized nanocellulose, the specific process is:

[0113] Take 3g of cotton fiber with a beating degree of 90, add 0.2g of cellulose complex enzyme and stir at 50℃ for 5h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 15min, filter it under reduced pressure and wash it with 200mL of deionized water, repeat 8 times to obtain pretreated fiber. Then add 1500mL of deionized water to the pretreated fiber and disperse it ultrasonically. Then add 0.03mol / g of 2,2,6,6-tetramethylpiperidinium nitrogen oxide and 0.6mol / g of NaBr, then add NaOH to adjust the pH of the reaction system to 10, then 150mL of NaClO (0.75 mol / g) solution dropwise (30 min to add), and continue stirring for 5h. After the reaction is completed, cool down and add hydrochloric acid to adjust the pH to neutral to obtain a suspension. After the suspension is filtered and washed with 1000mL of deionized water, repeat 8 times, and freeze-dry at -40℃ to obtain white powdery oxidized nanocellulose.

[0114] Step 2, preparation of lignocellulose, the specific process is:

[0115] Take 2g of brown cellulose, add 0.2g of cellulose complex enzyme and stir at 50℃ for 5h to pre-treat the fiber. After the reaction, inactivate it in an autoclave for 15 min, filter it under reduced pressure and wash it with 200mL of deionized water, repeat 8 times to obtain pre-treated brown cellulose. Further, use a high-pressure homogenizer to homogenize 80 times to obtain wood cellulose.

[0116] Step 3, preparation of double-anti-release PET support film, the specific process is as follows:

[0117] Preparation of double-antistatic substrate: First, take a 90 um thick PET film, and spin-coat a 5 um layer of antistatic coating I on the upper and lower surfaces of the PET respectively; then dry it at 120°C for later use.

[0118] Antistatic coating I: 5wt% of oxidized nanocellulose, 15wt% of waterborne polyurethane, 5wt% of cationic starch, 3wt% of isocyanate, 0.3wt% of wetting agent and 71.7wt% of water were mixed and stirred in a mixer at 600 r / min for 20 min to obtain the antistatic coating.

[0119] Preparation of double anti-release film: First, take a PET film with a thickness of 30 um, spin-coat a layer of 4 um antistatic coating II on the upper and lower surfaces of the PET, and then dry it at 100°C for use.

[0120] Antistatic coating II: 15wt% of waterborne polyurethane, 5wt% of cationic starch, 3wt% of isocyanate, 0.3wt% of wetting agent and 76.7wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0121] Preparation of double-anti-release PET support film: First, a layer of adhesive is spin-coated on the lower surface of the double-anti-release substrate to form a bonding layer with a thickness of 16 um and dried at 120°C. Then, it is compounded with the double-anti-release film, rolled up, and aged at 50°C for 60 hours to obtain the double-anti-release PET support film.

[0122] The adhesive composition of the bonding layer is as follows: 9wt% polyurethane, 9wt% polyvinyl alcohol, 9wt% silicon phosphate, 9wt% acrylate, 10wt% dimethyldivinylsilane, 9wt% epoxy acrylate, 15wt% acrylic acid, 10wt% N-dodecyldimethylamine, and 20%wt wood cellulose.

Claims

1. Preparation method of double-anti-release PET support film for OLED, Features: The specific steps include: Step 1, preparing oxidized nanocellulose; The specific process of step 1 is as follows: Step 1.1, taking 2g-3g of cotton fiber with a beating degree of 90, adding 0.1g-0.2g of cellulose complex enzyme and stirring at 35℃-50℃ for 3h~5h to pre-treat the fiber, inactivating it for 10min-15min after the reaction, filtering it and washing it with 100mL-200mL of deionized water, repeating 6~8 times to obtain pre-treated fiber; Step 1.2, adding 1000 mL-1500 mL of deionized water to the pretreated fiber obtained in step 1.1 and ultrasonically dispersing it, then adding 0.02 mol / g-0.03 mol / g of 2,2,6,6-tetramethylpiperidine nitrogen oxide and 0.4 mol / g-0.6 mol / g of NaBr, and then adding NaOH to adjust the pH of the reaction system to alkaline, and then adding 100 mL-150 mL of NaClO solution dropwise to the alkaline solution, continuing to stir for 3h-5h, and after the reaction is completed, adding hydrochloric acid to adjust the pH to neutral to obtain a suspension; Step 1.3, filtering the suspension prepared in step 1.2, washing with 500 mL-1000 mL of deionized water, repeating 6-8 times, and freeze-drying at -70°C to -40°C to obtain white powdery oxidized nanocellulose; Step 2, preparing lignocellulose; The specific process of step 2 is: Step 2.1, adding 0.1g-0.2g of cellulose complex enzyme to brown cellulose, and stirring at 35℃-50℃ for 3h~5h, inactivating in a sterilizing pot for 10-15min after the reaction, filtering and washing with 100-200mL of deionized water, repeating 6-8 times to obtain pretreated brown cellulose; Step 2.2, homogenizing the pretreated brown cellulose obtained in step 2.1 for 60-80 times to obtain lignocellulose; Step 3, preparing an antistatic coating I according to the oxidized nanocellulose prepared in step 1, and preparing an adhesive according to the wood cellulose prepared in step 2; In the step 3, the preparation process of the antistatic coating I is: The following components are weighed respectively by mass percentage: 2wt%-5wt% of oxidized nanocellulose, 10wt%-15wt% of aqueous polyurethane, 2wt%-5wt% of cationic starch, 0.1wt%-3wt% of isocyanate, 0.002wt%-0.3wt% of wetting agent, and the remaining component is water, and the sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an antistatic coating I is obtained; The preparation process of the adhesive is: The following components are weighed respectively by mass percentage: 5wt%-10wt% of polyurethane, 5wt%-10wt% of polyvinyl alcohol, 5wt%-10wt% of silicon phosphate, 5wt%-10wt% of acrylate, 5wt%-10wt% of dimethyl divinyl silane, 5wt%-10wt% of epoxy acrylate, 10wt%-20wt% of acrylic acid, 5wt%-10wt% of N-dodecyl dimethylamine, and 20wt%-30wt% of lignocellulose, and the sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an adhesive is obtained; Step 4, preparing a double-anti-release PET support film according to the antistatic coating II and the antistatic coating I prepared in step 3 and the adhesive; The specific process of step 4 is as follows: Step 4.1, take a PET film with a thickness of 60 um-90 um, and spin-coat a layer of 3um-5um antistatic coating I on the upper surface and the lower surface of the PET film respectively; then dry it at 80℃-120℃ to obtain a double-antistatic substrate for standby use; Step 4.2, take a PET film with a thickness of 20um-40um, spin-coat a layer of 3um-5um antistatic coating II on the upper surface and the lower surface of the PET film respectively, and then dry it at 80℃-120℃ to obtain a double anti-release film for standby use; Step 4.3, spin-coat a layer of adhesive on the lower surface of the double-anti-resistance substrate prepared in step 4.1 to form a bonding layer with a thickness of 13um-16um, and dry it at 80℃-120℃. Compound the double-anti-resistance substrate with the double-anti-resistance release film prepared in step 4.2 through the bonding layer, roll it up, and mature it at 40°C~50°C for 40h~60h to obtain a double-anti-resistance release PET support film.

2. The method for preparing the double-anti-release PET support film for OLED according to claim 1, Features: The preparation process of the antistatic coating II is: The following components are weighed respectively by mass percentage: 10wt%-15wt% waterborne polyurethane, 2wt%-5wt% cationic starch, 0.1wt%-3wt% isocyanate, 0.002wt%-0.3wt% wetting agent, and the remaining component is water. The sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, the antistatic coating II is obtained.

Citation Information

Patent Citations

  • Support film for OLED module and preparation method thereof

    CN112680135A

  • Antistatic coating, antistatic release film with high adhesion and stability and preparation method of antistatic release film

    CN113604088A

  • Nano-cellulose reinforced antistatic carrier tape paper and preparation process thereof

    CN116556112A

  • Preparation method of cellulose nano-paper-based MLCC release film

    CN116926980A