Defluorination adsorbent and preparation method thereof, and defluorination method for lithium battery recovery liquid
The hydrothermal method was used to synthesize calcium-based MOFs materials and prepare fluorine removal adsorbents, which solved the problem of high loss rate of nickel ions and cobalt ions in the lithium battery recycling solution, achieving efficient fluoride removal and reducing the waste of metal resources.
Patent Information
- Application Number
- CN202311455116.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-03
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-11-03
AI Technical Summary
When traditional adsorbents are used to remove fluoride from lithium battery recycling liquid, the loss rate of nickel ions and cobalt ions is too large, which seriously wastes the metal resources in the lithium battery recycling liquid.
Calcium-based MOFs materials are synthesized by hydrothermal method, and their structure and crystal form are adjusted using structural regulators to prepare fluoride removal adsorbents with excellent fluoride removal performance. Their adsorption performance and service life are improved through the granulation process.
It significantly reduces the loss of nickel ions and cobalt ions, increases the adsorption capacity and selectivity of fluoride ions, reduces mechanical wear and dissolution loss, and improves the performance and service life of the fluoride removal adsorbent.
Smart Images

Figure CN117563557B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium battery recycling, and in particular to a defluorination adsorbent and a preparation method thereof, and a defluorination method for lithium battery recycling liquid. Background Art
[0002] With the rapid development of the new energy industry, the demand for lithium batteries is gradually increasing. Lithium batteries are usually composed of structures such as positive electrodes, negative electrodes, electrolytes and diaphragms. Among them, the positive electrodes, negative electrodes and diaphragms often contain binders such as polyvinylidene fluoride (PVDF), which introduce corrosive fluorine elements and have a certain impact on the operation of the equipment. In order to avoid the waste of metal resources in lithium batteries, it is necessary to recycle and reuse metal elements with high added value after the lithium batteries are discarded. Usually, lithium batteries can be wet extracted to prepare lithium battery recovery liquid, and purified to obtain recovery products rich in metal elements. In addition to metal ions such as iron, cobalt and manganese, lithium battery recovery liquid also contains a certain amount of fluoride ions, which seriously affects the quality of the recovery product. Therefore, the lithium battery recovery liquid needs to be defluorinated.
[0003] The main methods for removing fluoride ions from solutions include extraction, precipitation and adsorption. Among them, the adsorption method is widely used due to its advantages of simple operation, low cost, safety and effectiveness. At present, different types of adsorbents have been developed, such as natural mineral materials, carbon materials, metal oxide materials, metal hydroxide materials and metal-organic frameworks (MOFs) materials. However, when traditional adsorbents are used to remove fluoride from lithium battery recycling liquid, the loss rate of nickel ions and cobalt ions is too large, which seriously wastes the metal resources in the lithium battery recycling liquid. Summary of the invention
[0004] Based on this, it is necessary to provide a defluorination adsorbent and a preparation method thereof and a defluorination method for lithium battery recovery liquid to solve the problem that when traditional adsorbents are used to defluorinate lithium battery recovery liquid, the loss rate of nickel ions and cobalt ions is too large, which seriously wastes the metal resources in the lithium battery recovery liquid.
[0005] The above object of the present invention is achieved through the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a defluorination adsorbent, comprising the following steps:
[0007] Mixing calcium salt, structure regulator and fumaric acid, and performing hydrothermal reaction to prepare calcium-based MOFs material;
[0008] Mixing the calcium-based MOFs material, a binder and an organic solvent to prepare a slurry;
[0009] The slurry is granulated to prepare the defluorination adsorbent.
[0010] In one embodiment, the structure modifier includes one or more of formic acid, acetic acid, oxalic acid, propionic acid, butyric acid, valeric acid, caproic acid, benzoic acid, diphenyl dicarboxylic acid, terephthalic acid, isophthalic acid and phthalic acid.
[0011] In one embodiment, the calcium salt includes one or more of calcium chloride, calcium sulfate, calcium gluconate, calcium hydrogen phosphate, calcium dihydrogen phosphate, calcium nitrate, calcium bicarbonate, calcium hydrogen sulfate, calcium bisulfite and calcium permanganate.
[0012] In one embodiment, one or more of the following conditions are met:
[0013] (1) The molar ratio of the calcium salt, the structure regulator and the fumaric acid is 1:(1-5):(1-5);
[0014] (2) The temperature of the hydrothermal reaction is 20°C to 40°C;
[0015] (3) The hydrothermal reaction time is 18h~28h.
[0016] In one embodiment, mixing calcium salt, structure modifier and fumaric acid comprises the following steps:
[0017] Mixing the calcium salt, the structure regulator and water to prepare a first mixed solution;
[0018] The fumaric acid is added to the first mixed solution to prepare a second mixed solution.
[0019] In one embodiment, after the hydrothermal reaction, the following steps are further included:
[0020] The third mixed solution containing the calcium-based MOFs material is purified, wherein the purification process includes one or more of a centrifugal process, a washing process and a drying process.
[0021] In one embodiment, after the drying process, the following steps are further included:
[0022] The calcium-based MOFs material is crushed and sieved to make the particle size of the calcium-based MOFs material ≤150 μm.
[0023] In one embodiment, one or more of the following conditions are met:
[0024] (1) The binder includes one or more of polydimethyldiallyl ammonium chloride, polyacrylonitrile, polyvinylidene fluoride, polyvinyl chloride, epoxy resin and sodium alginate;
[0025] (2) The organic solvent includes one or more of N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone and N,N-dimethylformamide;
[0026] (3) The mass ratio of the calcium-based MOFs material, the binder and the organic solvent is 1:(0.1-0.8):(3-6).
[0027] In a second aspect, the present invention provides a defluorination adsorbent, which is prepared by the above-mentioned preparation method of the defluorination adsorbent.
[0028] In one embodiment, the defluorination adsorbent satisfies one or more of the following conditions:
[0029] (1) The particle size of the defluorination adsorbent is 0.3 mm to 0.7 mm;
[0030] (1) The porosity of the defluorination adsorbent is 20% to 45%;
[0031] (2) The saturated adsorption capacity of the defluorination adsorbent for fluoride ions is 100 mmol / g to 400 mmol / g;
[0032] (3) The mass fraction of the calcium-based MOFs material in the defluorination adsorbent is 60% to 80%.
[0033] In a third aspect, the present invention provides a method for removing fluorine from lithium battery recovery liquid, comprising the following steps:
[0034] The above-mentioned defluorination adsorbent is used to defluorinate the lithium battery recovery liquid.
[0035] The present invention has the following beneficial effects:
[0036] The present invention synthesizes calcium-based MOFs materials by a simple one-step hydrothermal method. Compared with other MOFs materials, calcium-based MOFs materials have stronger coordination ability for fluoride ions, but weaker coordination ability for nickel ions and cobalt ions, so that calcium-based MOFs materials show excellent defluorination performance and can significantly reduce the loss of nickel ions and cobalt ions. By using a structural regulator, the structure and crystal form of the calcium-based MOFs material can be adjusted to expose more fluoride ion adsorption sites, thereby increasing the adsorption capacity and adsorption selectivity of the calcium-based MOFs material for fluoride ions. At the same time, the calcium-based MOFs material is made into a defluorination adsorbent through a granulation process, which can reduce its mechanical wear and dissolution loss, and improve the adsorption performance and service life of the defluorination adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The physical pictures of product A in Example 1 before and after granulation;
[0038] Figure 2 XRD patterns of calcium-based MOFs materials of Examples 1 to 3;
[0039] Figure 3 Schematic diagram of the spatial structure of calcium-based MOFs materials. DETAILED DESCRIPTION
[0040] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0043] At present, the main methods for removing fluoride ions from lithium battery recycling liquid include extraction, precipitation and adsorption. Among them, the extraction method uses an extractant to extract the lithium battery recycling liquid to achieve the separation of metal ions and fluoride ions, but a certain amount of extractant will remain in the lithium battery recycling liquid after extraction, resulting in a decrease in the quality of the recovered product; at the same time, fluoride ions will remain in the extract, resulting in cumbersome subsequent processing steps for the extract, high cost, difficult to recycle and reuse, and not suitable for industrial application. The precipitation method usually uses calcium salt to react with fluoride ions to form CaF 2 Sedimentation is mainly used for the pretreatment of high-concentration fluoride-containing wastewater, but the precipitation method has poor fluoride removal effect and requires secondary treatment using other fluoride removal processes. In addition, the amount of sludge produced is large, which can easily cause secondary pollution.
[0044] The adsorption method utilizes the selective adsorption of fluoride ions by adsorbents to remove fluoride ions from lithium battery recovery liquid. It is widely used due to its advantages of low cost, simple process, and high defluorination efficiency. It has been reported that alumina, aluminum hydroxide, or soluble aluminum salts are used as defluoridants. Defluoridants are added to fluorine-containing nickel-cobalt-manganese solutions, and acid and alkali solutions are added to adjust the pH. The fluoride-containing filtrate and nickel-cobalt-manganese filter residue are obtained by filtration. However, this defluorination process requires the use of alkali solution, which results in excessive loss of metal ions such as nickel, cobalt, and manganese due to local over-alkalinity or entrainment, and Na will be introduced during the defluorination process. + or K + Alkali metal ions such as ions seriously reduce the quality and performance of the recovered products.
[0045] Among many adsorbents, metal-organic frameworks (MOFs) materials have attracted much attention due to their adjustable pore structure, large specific surface area, high structural diversity, and rich active sites. Among them, the MOFs materials used for adsorbing fluoride ions mainly include aluminum-based MOFs (MIL-96), iron-based MOFs (MIL-88A), and zirconium-based MOFs (MOF-801 and UiO-66). However, these MOFs materials still have the problem of serious metal ion loss when defluoridating lithium battery recycling liquid.
[0046] Therefore, it is necessary to find a defluorination adsorbent that can efficiently remove fluoride ions from lithium battery recovery liquid and effectively reduce the loss of metal elements such as nickel, cobalt, and manganese.
[0047] Based on this, the first aspect of the present invention provides a method for preparing a defluorination adsorbent to solve the problem that when traditional adsorbents are used to defluorinate lithium battery recovery liquid, the loss rate of nickel ions and cobalt ions is too large, which seriously wastes the metal resources in the lithium battery recovery liquid.
[0048] In some embodiments, the method for preparing a defluorination adsorbent comprises the following steps:
[0049] Mixing calcium salt, structure regulator and fumaric acid, and performing hydrothermal reaction to prepare calcium-based MOFs material;
[0050] Mixing calcium-based MOFs materials, a binder and an organic solvent to prepare a slurry;
[0051] The slurry is granulated to prepare a defluorination adsorbent.
[0052] Understandably, fumaric acid, also known as fumaric acid, fumaric acid and corydalic acid, has a chemical formula of C 4 H 4 O 4, which can act as a bidentate ligand to coordinate with calcium ions to form calcium-based MOFs materials.
[0053] The present invention synthesizes calcium-based MOFs materials by a simple one-step hydrothermal method. Compared with other MOFs materials, calcium-based MOFs materials have stronger coordination ability for fluoride ions, but weaker coordination ability for nickel ions and cobalt ions, so that calcium-based MOFs materials show excellent defluorination performance and can significantly reduce the loss of nickel ions and cobalt ions. By using a structural regulator, the structure and crystal form of the calcium-based MOFs material can be adjusted to expose more fluoride ion adsorption sites, thereby increasing the adsorption capacity and adsorption selectivity of the calcium-based MOFs material for fluoride ions. At the same time, the calcium-based MOFs material is made into a defluorination adsorbent through a granulation process, which can reduce its mechanical wear and dissolution loss, and improve the adsorption performance and service life of the defluorination adsorbent.
[0054] Different binders have different hydrophilicities and different ion mass transfer efficiencies in the solution. Selecting a suitable binder can improve the hydrophilicity and ion mass transfer efficiency of the defluorination adsorbent, making it exhibit better adsorption effects. In addition, compared with metal ions such as aluminum, iron, zirconium, cerium and lanthanum, calcium ions are easy to obtain, low cost, and have a larger ionic radius and higher charge density. They can form stable coordination bonds with fumaric acid. Therefore, calcium-based MOFs materials have good structural stability and can maintain their structural integrity over a wide range of temperature and humidity, thereby exhibiting better adsorption and storage performance.
[0055] Optionally, the structure regulator includes one or more mixtures of formic acid, acetic acid, oxalic acid, propionic acid, butyric acid, valeric acid, caproic acid, benzoic acid, biphenyl dicarboxylic acid, terephthalic acid, isophthalic acid and phthalic acid. Further optionally, the structure regulator includes one or more of formic acid, oxalic acid, propionic acid, butyric acid, valeric acid and caproic acid. Preferably, the structure regulator is formic acid.
[0056] Using carboxylic acid compounds such as formic acid, oxalic acid and propionic acid as structural regulators can adjust the pH and other conditions of the hydrothermal reaction, affect the coordination reaction between fumaric acid and calcium ions, and regulate the crystal form and structure of calcium-based MOFs. Introducing structural regulators during the hydrothermal reaction is conducive to improving the porosity and specific surface area of calcium-based MOFs materials, exposing more fluoride ion adsorption sites, thereby increasing the selective adsorption capacity of fluoride ions.
[0057] Optionally, the calcium salt comprises calcium chloride (CaCl 2 ), calcium sulfate (CaSO 4 ), calcium gluconate (C 12 H 22 O 14 Ca), calcium hydrogen phosphate (CaHPO 4), monocalcium phosphate (Ca(H 2 PO 4 ) 2 ), calcium nitrate (Ca(NO 3 ) 2 ), calcium bicarbonate (Ca(HCO 3 ) 2 ), calcium hydrogen sulfate (Ca(HSO 4 ) 2 ), calcium bisulfite (Ca(HSO 3 ) 2 ) and calcium permanganate (Ca(MnO 4 ) 2 ) or more. Further optionally, the calcium salt includes calcium chloride (CaCl 2 ), calcium sulfate (CaSO 4 ), calcium gluconate (C 12 H 22 O 14 Ca) and calcium nitrate (Ca(NO 3 ) 2 ) or more. Preferably, the calcium salt comprises calcium chloride (CaCl 2 ) or calcium sulfate (CaSO 4 ).
[0058] It is understandable that the calcium salt may be a calcium salt without bound water, such as anhydrous calcium chloride and anhydrous calcium sulfate; the calcium salt may also be a calcium salt containing bound water, such as calcium chloride dihydrate (CaCl 2 ·2H 2 O) and calcium nitrate tetrahydrate (Ca(NO 3 ) 2 ·4H 2 O) etc.
[0059] Optionally, the molar ratio of calcium salt, structure regulator and fumaric acid is 1: (1-5): (1-5). It is understandable that the molar ratio of calcium salt and structure regulator can be 1: 1, 1: 1.5, 1: 2, 1: 2.5, 1: 3, 1: 3.5, 1: 4, 1: 4.5, 1: 5; the molar ratio of calcium salt and fumaric acid can be 1: 1, 1: 1.5, 1: 2, 1: 2.5, 1: 3, 1: 3.5, 1: 4, 1: 4.5, 1: 5. Further optionally, the molar ratio of calcium salt, structure regulator and fumaric acid is 1: (1-3): (1-3). Preferably, the molar ratio of calcium salt, structure regulator and fumaric acid is 1: 1.5: 1.
[0060] Optionally, the temperature of the hydrothermal reaction is 20°C to 40°C, including but not limited to: 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C. Further optionally, the temperature of the hydrothermal reaction is 30°C to 40°C. Preferably, the temperature of the hydrothermal reaction is 40°C.
[0061] Optionally, the hydrothermal reaction time is 18h~28h, including but not limited to: 18h, 19h, 20h, 21h, 22h, 23h, 24h, 25h, 26h, 27h, 28h. Further optionally, the hydrothermal reaction time is 20h~24h. Preferably, the hydrothermal reaction time is 24h.
[0062] When synthesizing calcium-based MOFs materials by hydrothermal reaction, lower reaction temperature and longer reaction time will lead to lower yield; at the same time, lower reaction temperature can improve the selectivity of calcium-based MOFs materials, avoid or reduce the occurrence of side reactions, inhibit the formation of impurities, and thus improve the purity of the product; in addition, lower reaction temperature is also conducive to the formation of calcium-based MOFs materials with smaller pore size or shorter chain length, improving their adsorption performance. Controlling the temperature of the hydrothermal reaction at 20℃~40℃ and the time at 20℃~40℃ can achieve a balance between yield, purity and adsorption performance, and prepare calcium-based MOFs materials with high yield, high purity and high adsorption.
[0063] In some embodiments, mixing the calcium salt, the structure modifier, and fumaric acid comprises the following steps:
[0064] Mixing calcium salt, structure regulator and water to prepare a first mixed solution;
[0065] The second mixed solution is prepared by adding fumaric acid to the first mixed solution.
[0066] By adding materials in steps and controlling the temperature and time when mixing the three raw materials, the raw materials can be mixed more evenly, which is beneficial to the morphology control of calcium-based MOFs materials and improves the reaction rate and product purity.
[0067] Optionally, the concentration of calcium ions in the second mixed solution is 150mmoL / L~500mmoL / L, including but not limited to: 150mmoL / L, 200mmoL / L, 250mmoL / L, 300mmoL / L, 350mmoL / L, 400mmoL / L, 450mmoL / L, 500mmoL / L. Further optionally, the concentration of calcium ions in the second mixed solution is 150mmoL / L~300mmoL / L. Preferably, the concentration of calcium ions in the second mixed solution is 150mmoL / L.
[0068] Optionally, the concentration of fumaric acid in the second mixed solution is 0.75moL / L~2.5moL / L, including but not limited to: 0.75moL / L, 1moL / L, 1.25moL / L, 1.5moL / L, 1.75moL / L, 2moL / L, 2.25moL / L, 2.5moL / L. Further optionally, the concentration of fumaric acid in the second mixed solution is 0.75moL / L~1moL / L. Preferably, the concentration of fumaric acid in the second mixed solution is 0.75moL / L.
[0069] Optionally, the pH of the second mixed solution is 2-7, including but not limited to: 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7. Further optionally, the pH of the second mixed solution is 2-4.
[0070] Optionally, the temperature of the mixed calcium salt, structure regulator and water is 20°C to 40°C, including but not limited to: 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C. Further optionally, the temperature of the mixed calcium salt, structure regulator and water is 25°C to 35°C. Preferably, the temperature of the mixed calcium salt, structure regulator and water is 30°C.
[0071] Optionally, the time for mixing calcium salt, structure regulator and water is 0.1h~1h, including but not limited to: 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h. Further optionally, the time for mixing calcium salt, structure regulator and water is 0.2h~0.6h. Preferably, the time for mixing calcium salt, structure regulator and water is 0.5h.
[0072] In some embodiments, after the hydrothermal reaction, the method further comprises the following steps:
[0073] The third mixed solution containing the calcium-based MOFs material is purified, wherein the purification process includes one or more of a centrifugal process, a washing process and a drying process.
[0074] Optionally, the temperature of the drying process is 80°C to 160°C, including but not limited to: 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C. Further optionally, the temperature of the drying process is 80°C to 100°C. Preferably, the temperature of the drying process is 90°C.
[0075] Optionally, the drying time is 12h~24h, including but not limited to: 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h. Further optionally, the drying time is 12h~18h. Preferably, the drying time is 12h.
[0076] Further optionally, after the hydrothermal reaction, the method further includes the following steps: centrifuging, washing and drying the third mixed solution containing the calcium-based MOFs material.
[0077] Optionally, after the drying process, the method further comprises the following steps: crushing and sieving the calcium-based MOFs material to make the particle size of the calcium-based MOFs material ≤150 μm. Further, optionally, the particle size of the calcium-based MOFs material ≤50 μm.
[0078] In some specific embodiments, after the drying treatment, the following steps are also included: using a crusher to crush the calcium-based MOFs material, and using a 100-mesh to 300-mesh sieve to sieve the calcium-based MOFs material to make the particle size of the calcium-based MOFs material ≤150 μm.
[0079] Optionally, the method of mixing the calcium-based MOFs material, the binder and the organic solvent is a mechanical stirring method; wherein the rotation speed of the mechanical stirring method is 300rpm~500rpm, including but not limited to: 300rpm, 350rpm, 400rpm, 450rpm, 500rpm.
[0080] Optionally, the slurry is subjected to a granulation treatment, comprising the following steps: transferring the slurry into a syringe, and using the syringe to drop the slurry into water drop by drop to form granules.
[0081] Optionally, the binder includes one or more of polydimethyldiallyl ammonium chloride (PDDA), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinyl chloride (PVC), epoxy resin and sodium alginate. Further optionally, the binder includes one or more of polydimethyldiallyl ammonium chloride (PDDA) and polyacrylonitrile (PAN).
[0082] Calcium-based MOFs materials are usually in powder form, with low structural strength, prone to mechanical wear and effective component dissolution, which reduces their adsorption capacity, adsorption selectivity and service life. Compounding calcium-based MOFs materials with binders and granulating them can increase their physical strength, reduce mechanical wear and effective component dissolution, improve their adsorption performance and service life, and make them easy to recycle and reuse, without affecting the subsequent treatment of lithium battery recovery liquid.
[0083] Optionally, the organic solvent includes one or more of N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF). Further optionally, the organic solvent includes one or more of N,N-dimethylacetamide (DMAC) and dimethyl sulfoxide (DMSO).
[0084] Optionally, the mass ratio of calcium-based MOFs material, binder and organic solvent is 1: (0.1-0.8): (3-6). It can be understood that the mass ratio of calcium-based MOFs material and binder can be 1: 0.1, 1: 0.2, 1: 0.3, 1: 0.4, 1: 0.5, 1: 0.6, 1: 0.7, 1: 0.8; the mass ratio of calcium-based MOFs material and organic solvent can be 1: 3, 1: 3.5, 1: 4, 1: 4.5, 1: 5, 1: 5.5, 1: 6. Further optionally, the mass ratio of calcium-based MOFs material, binder and organic solvent is 1: (0.1-0.4): (3-4). Preferably, the mass ratio of calcium-based MOFs material, binder and organic solvent is 1: 0.2: 3.
[0085] In a second aspect, the present invention provides a defluorination adsorbent, which is prepared by the above-mentioned preparation method of the defluorination adsorbent.
[0086] Optionally, the particle size of the defluorination adsorbent is 0.3mm~0.7mm, including but not limited to: 0.3mm, 0.35mm, 0.4mm, 0.45mm, 0.5mm, 0.55mm, 0.6mm, 0.65mm, 0.7mm. Further optionally, the particle size of the defluorination adsorbent is 0.5mm~0.6mm. It can be understood that the particle size refers to the size of the particles obtained by granulation, which can be the diameter of spherical particles, or the equivalent circle diameter of spherical particles, strip particles or irregular particles. If the particle size of the defluorination adsorbent is too low, its use resistance is large and it is not easy to recover; if the particle size of the defluorination adsorbent is too large, its specific surface area is small and the adsorption efficiency is low.
[0087] Optionally, the porosity of the defluorination adsorbent is 20% to 45%, including but not limited to: 20%, 25%, 30%, 35%, 40%, 45%. Further optionally, the porosity of the defluorination adsorbent is 30% to 40%.
[0088] Optionally, the saturated adsorption capacity of the defluorination adsorbent for fluoride ions is 100mmol / g to 400mmol / g, including but not limited to: 100mmol / g, 150mmol / g, 200mmol / g, 250mmol / g, 300mmol / g, 350mmol / g, 400mmol / g. The saturated adsorption capacity of the defluorination adsorbent for fluoride ions is 300mmol / g to 400mmol / g.
[0089] Optionally, the mass fraction of the calcium-based MOFs material in the defluorination adsorbent is 60% to 80%, including but not limited to: 60%, 65%, 70%, 75%, 80%. Further optionally, the mass fraction of the calcium-based MOFs material in the defluorination adsorbent is 65% to 75%.
[0090] In a third aspect, the present invention provides a method for defluorinating lithium battery recovery liquid, which is the application of the above-mentioned defluorinating adsorbent in the field of lithium battery recovery.
[0091] In some embodiments, the method for removing fluorine from lithium battery recovery liquid comprises the following steps:
[0092] The above-mentioned defluorination adsorbent is used to defluorinate the lithium battery recovery liquid.
[0093] Optionally, the dosage of the defluorination adsorbent is 1g / L~50g / L, including but not limited to: 1g / L, 5g / L, 10g / L, 15g / L, 20g / L, 25g / L, 30g / L, 35g / L, 40g / L, 45g / L, 50g / L.
[0094] Optionally, the temperature of the defluorination treatment is 20°C~30°C, including but not limited to: 20°C, 22°C, 24°C, 26°C, 28°C, 30°C.
[0095] It can be understood that the time of defluorination treatment takes into account the content of each component of the lithium battery recovery liquid, the treatment volume of the lithium battery recovery liquid, the amount of defluorination adsorbent, the temperature of the defluorination treatment, etc. Optionally, the time of defluorination treatment is 3h~6h, including but not limited to: 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h.
[0096] The present invention is further described in detail below with reference to specific embodiments.
[0097] In the following specific embodiments and comparative examples, the raw materials used, unless otherwise specified, are all commercially available products; the instruments used, unless otherwise specified, are all commercially available products; and the processes used, unless otherwise specified, are all routinely selected by those skilled in the art.
[0098] Example 1
[0099] (1) Calcium chloride, formic acid and water were placed in a round-bottom flask and stirred at 30°C for 0.5 h to obtain a first mixed solution; fumaric acid was added to the first mixed solution to obtain a second mixed solution; the second mixed solution was stirred at 40°C for 24 h for hydrothermal reaction to obtain a third mixed solution containing a white solid. The molar ratio of calcium chloride, formic acid and fumaric acid was 1:1.5:1, the concentration of calcium salt was 150 mmol / L, the concentration of fumaric acid was 0.75 mol / L, and the pH of the second mixed solution was 2-4.
[0100] (2) The third mixed liquid is centrifuged to obtain a white solid; the white solid is washed multiple times with ethanol and pure water, and placed in a constant temperature drying oven to dry at 90° C. for 12 h; the dried white solid is ground into powder with a pulverizer, and passed through a 200-mesh sieve to obtain a calcium-based MOFs material with a particle size of ≤75 μm.
[0101] (3) Add polydimethyldiallylammonium chloride (PDDA) and N,N-dimethylacetamide (DMAC) to the calcium-based MOFs material, and mechanically stir the mixture at 400 rpm to prepare a uniform slurry; wherein the mass ratio of the calcium-based MOFs material, PDDA and PDDA is 1:0.2:3.
[0102] (4) Transfer the slurry into a syringe and drip it into water drop by drop to form particles, which are recorded as Product A.
[0103] Example 2
[0104] (1) Calcium chloride, formic acid and water were placed in a round-bottom flask and stirred at 30°C for 0.5 h to obtain a first mixed solution; fumaric acid was added to the first mixed solution to obtain a second mixed solution; the second mixed solution was stirred at 40°C for 24 h for hydrothermal reaction to obtain a third mixed solution containing a white solid. The molar ratio of calcium chloride, formic acid and fumaric acid was 1:1.5:1, the concentration of calcium salt was 150 mmol / L, the concentration of fumaric acid was 0.75 mol / L, and the pH of the second mixed solution was 2-4.
[0105] (2) The third mixed liquid is centrifuged to obtain a white solid; the white solid is washed multiple times with ethanol and pure water, and placed in a constant temperature drying oven to dry at 90° C. for 12 h; the dried white solid is ground into powder with a pulverizer, and passed through a 200-mesh sieve to obtain a calcium-based MOFs material with a particle size of ≤75 μm.
[0106] (3) Add polyacrylonitrile (PAN) and dimethyl sulfoxide (DMSO) to the calcium-based MOFs material, and mechanically stir the mixture at a speed of 400 rpm to prepare a uniform slurry; wherein the mass ratio of the calcium-based MOFs material, PAN, and DMSO is 1:0.2:3.
[0107] (4) Transfer the slurry into a syringe and drip it into water drop by drop to form particles, which are recorded as product B.
[0108] Example 3
[0109] (1) Calcium sulfate, formic acid and water were placed in a round-bottom flask and stirred at 30°C for 0.5 h to obtain a first mixed solution; fumaric acid was added to the first mixed solution to obtain a second mixed solution; the second mixed solution was stirred at 40°C for 24 h for hydrothermal reaction to obtain a third mixed solution containing a white solid. The molar ratio of calcium sulfate, formic acid and fumaric acid was 1:1.5:1, the concentration of calcium salt was 150 mmol / L, the concentration of fumaric acid was 0.75 mol / L, and the pH of the second mixed solution was 2-4.
[0110] (2) The third mixed liquid is centrifuged to obtain a white solid; the white solid is washed multiple times with ethanol and pure water, and placed in a constant temperature drying oven to dry at 90° C. for 12 h; the dried white solid is ground into powder with a pulverizer, and passed through a 200-mesh sieve to obtain a calcium-based MOFs material with a particle size of ≤75 μm.
[0111] (3) Add polydimethyldiallylammonium chloride (PDDA) and N,N-dimethylacetamide (DMAC) to the calcium-based MOFs material, and mechanically stir the mixture at 400 rpm to prepare a uniform slurry; wherein the mass ratio of the calcium-based MOFs material, PDDA and PDDA is 1:0.2:3.
[0112] (4) Transfer the slurry into a syringe and drip it into water drop by drop to form particles, which are recorded as product C.
[0113] Example 4
[0114] The difference between this embodiment and embodiment 1 is that the temperature of the hydrothermal reaction is 60° C., and the obtained defluorination adsorbent is recorded as product D.
[0115] Example 5
[0116] The difference between this embodiment and embodiment 1 is that the molar ratio of calcium chloride, formic acid and fumaric acid is 1:0.5:1, and the obtained defluorination adsorbent is recorded as product E.
[0117] Example 6
[0118] The difference between this embodiment and embodiment 1 is that calcium chloride, formic acid and fumaric acid are mixed simultaneously, and the obtained defluorination adsorbent is recorded as product F.
[0119] Comparative Example 1
[0120] The difference between this comparative example and Example 1 is that no formic acid is used and the obtained defluorination adsorbent is recorded as Product G.
[0121] Comparative Example 2
[0122] The difference between this comparative example and Example 1 is that calcium chloride is replaced by ferric chloride, and the obtained defluorination adsorbent is recorded as product H.
[0123] Comparative Example 3
[0124] This comparative example uses a commercially available defluorination adsorbent, which is recorded as Product I.
[0125] Test Case
[0126] (1) The actual picture of product A in Example 1 before and after granulation is as follows Figure 1 As shown. Figure 1 It can be seen that the calcium-based MOFs material prepared in Example 1 is in the form of a white powder. After granulation, the product A is spherical particles with a particle size of 0.5 mm to 0.6 mm, a porosity of 38%, and a saturated adsorption capacity for fluoride ions of 316 mmol / g.
[0127] (2) XRD test was performed on the calcium-based MOFs materials of Examples 1 to 3. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that there is a weak diffraction peak at 2θ of 30°~35°, indicating that the calcium-based MOFs materials of Examples 1~3 all contain calcium elements. The schematic diagram of their spatial structure is shown in Figure 3 shown.
[0128] (3) Prepare electrolyte waste liquid with a fluoride ion content of 200 ppm, a cobalt ion content of 7000 ppm, and a nickel ion content of 8000 ppm; take 10 mL of the product and load it into a resin column, add 100 mL of electrolyte waste liquid for adsorption test, and the flow rate is 2 BV / h; pass the effluent of the resin column through a 0.45 μm microfiltration membrane, and test the fluoride ion, cobalt ion and nickel ion contents of the effluent. The results are shown in Table 1.
[0129] Table 1. Comparison of adsorption performance of products
[0130]
[0131] As shown in Table 1, Product I is a commercially available defluorination adsorbent, and its fluoride ion adsorption rate can reach more than 99%, but it also adsorbs more cobalt ions and nickel ions. The cobalt ion adsorption rate reaches 22.33%, and the nickel ion adsorption rate reaches 44.6%. The metal ion loss is very serious.
[0132] In comparison, the fluoride ion adsorption rate of products A~F is ≥60.70%, the cobalt ion adsorption rate is ≤10.17%, and the nickel ion adsorption rate is ≤15.71%, indicating that the defluorination adsorbent containing calcium-based MOFs materials not only shows excellent defluorination performance, but also can reduce the loss of nickel and cobalt ions. Among them, the fluoride ion adsorption rate of products A and B made with calcium chloride as raw materials is 100%, and the defluorination performance is even better. Product B uses PAN as a binder, which changes the hydrophilicity and ion mass transfer efficiency of the defluorination adsorbent, and the adsorption amount of metal ions is lower, which can further reduce metal loss. Product C uses calcium sulfate as raw material, and the defluorination performance is slightly reduced. The hydrothermal temperature of product D increases from 30℃ to 60℃, and the adsorption amount of metal ions is higher. It may be that the increase in hydrothermal temperature leads to an increase in the yield of calcium-based MOFs materials. Considering the energy consumption problem of industrial applications, it can be used as an alternative. Product E reduces the amount of formic acid added, which is not conducive to the morphology control of calcium-based MOFs materials, and the defluorination performance is slightly reduced. The three raw materials of product F are mixed at the same time, which affects the morphology and purity of the calcium-based MOFs material and has a certain negative impact on the fluorine removal performance.
[0133] Product G did not use formic acid, and the fluoride ion adsorption rate was only 38.2%, with extremely poor defluorination performance. Product H changed the central metal ion of the MOFs material, and had a good adsorption effect on fluoride ions, cobalt ions, and nickel ions, but the loss of metal ions was very serious.
[0134] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0135] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A method for preparing a defluorination adsorbent, characterized in that: The following steps are involved: Mixing calcium salt, structure regulator and fumaric acid, and performing hydrothermal reaction to prepare calcium-based MOFs material; Mixing the calcium-based MOFs material, a binder and an organic solvent to prepare a slurry; granulating the slurry to prepare the defluorination adsorbent; The molar ratio of the calcium salt, the structure regulator and the fumaric acid is 1:(1-5):(1-5); The temperature of the hydrothermal reaction is 20°C to 40°C; The hydrothermal reaction time is 18h to 28h; The saturated adsorption capacity of the defluorination adsorbent for fluoride ions is 100 mmol / g to 400 mmol / g.
2. The method for preparing a defluorination adsorbent according to claim 1, characterized in that: The structure regulator includes one or more of formic acid, acetic acid, oxalic acid, propionic acid, butyric acid, valeric acid, caproic acid, benzoic acid, diphenyl dicarboxylic acid, terephthalic acid, isophthalic acid and phthalic acid.
3. The method for preparing a defluorination adsorbent according to claim 2, characterized in that: The calcium salt includes one or more of calcium chloride, calcium sulfate, calcium gluconate, calcium hydrogen phosphate, calcium dihydrogen phosphate, calcium nitrate, calcium hydrogen carbonate, calcium hydrogen sulfate, calcium hydrogen sulfite and calcium permanganate.
4. The method for preparing a defluorination adsorbent according to any one of claims 1 to 3, characterized in that: Mixing the calcium salt, the structure modifier and the fumaric acid comprises the following steps: Mixing the calcium salt, the structure regulator and water to prepare a first mixed solution; The fumaric acid is added to the first mixed solution to prepare a second mixed solution.
5. The method for preparing a defluorination adsorbent according to claim 4, characterized in that: After the hydrothermal reaction, the method further comprises the following steps: The third mixed solution containing the calcium-based MOFs material is purified, wherein the purification process includes one or more of a centrifugal process, a washing process and a drying process.
6. The method for preparing a defluorination adsorbent according to claim 5, characterized in that: After the drying process, the method further comprises the following steps: The calcium-based MOFs material is crushed and sieved to make the particle size of the calcium-based MOFs material ≤150 μm.
7. The method for preparing a defluorination adsorbent according to any one of claims 1 to 3, characterized in that: One or more of the following conditions are met: (1) The binder includes one or more of polydimethyldiallyl ammonium chloride, polyacrylonitrile, polyvinylidene fluoride, polyvinyl chloride, epoxy resin and sodium alginate; (2) The organic solvent includes one or more of N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone and N,N-dimethylformamide; (3) The mass ratio of the calcium-based MOFs material, the binder and the organic solvent is 1:(0.1-0.8):(3-6).
8. A defluorination adsorbent, characterized in that: The defluorination adsorbent is prepared by the preparation method of the defluorination adsorbent as described in any one of claims 1 to 7.
9. The defluorination adsorbent according to claim 8, characterized in that: The defluorination adsorbent meets one or more of the following conditions: (1) The particle size of the defluorination adsorbent is 0.3 mm to 0.7 mm; (2) The porosity of the defluorination adsorbent is 20% to 45%; (3) The mass fraction of the calcium-based MOFs material in the defluorination adsorbent is 60% to 80%.
10. A method for removing fluorine from lithium battery recovery liquid, characterized in that: The following steps are involved: The defluorination adsorbent as described in claim 8 or 9 is used to defluorinate the lithium battery recovery liquid.