A hydraulic concrete low-temperature melting anti-abrasion repair protective layer and its construction method

By using low-temperature melting technology to sinter a mixture of potassium oxide, alumina and mineral fillers on the surface of hydraulic concrete, a ceramic protective layer is formed, which solves the problem of insufficient abrasion resistance of hydraulic concrete buildings and achieves efficient protective effects and Good combination performance.

CN117567176BActive Publication Date: 2024-10-22NANJING HYDRAULIC RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311651709.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2024-10-22
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

Existing hydraulic concrete buildings have insufficient abrasion resistance after abrasion damage, and existing protective layer materials have problems such as limited abrasion resistance, weak bonding ability with the base concrete, and difficulty in maintaining integrity.

Method used

Low-temperature melting technology is used to evenly cover the concrete surface with a mixture of water, potassium oxide, alumina and mineral fillers, and is sintered by a flame spray gun to form a ceramic anti-abrasion repair protective layer to enhance the anti-abrasion and anti-corrosion properties of the concrete. .

Benefits of technology

It significantly improves the abrasion resistance and anti-corrosion properties of hydraulic concrete, forms an overall protective layer that is well bonded with the concrete, enhances the wear resistance and protection capabilities of the concrete, and is simple to construct and the material is green and non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a low-temperature melting wear-resistant repair and protection layer for hydraulic concrete and a construction method thereof. The repair and protection material is a mixture of water, potassium oxide, silicon dioxide and aluminum oxide, which is evenly covered on the concrete surface, and then sintered on the concrete surface by low-temperature melting technology to form a sintered wear-resistant repair and protection layer, at which time the concrete and the repair and protection material form a whole; the components in the mixture are mixed in the following mass proportions: 10 to 25 parts of water, 1.30 to 1.63 parts of potassium oxide, 4.0 to 4.5 parts of silicon dioxide, and 1 to 1.2 parts of aluminum oxide. The repair and protection layer has excellent anti-abrasion and anti-corrosion properties, can effectively improve the anti-abrasion ability of hydraulic concrete, significantly improve the anti-abrasion ability of concrete, extend the service life of hydraulic concrete, reduce the secondary maintenance cost of hydraulic concrete in the later stage, and the production method is simple and convenient, and is suitable for new and old hydraulic concrete structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydraulic concrete materials and relates to a method for preparing an anti-abrasion repair protective layer of hydraulic anti-abrasion concrete. Background Art

[0002] Abrasion resistance is one of the important properties of hydraulic concrete structures. Hydraulic concrete structures are subjected to abrasion and cavitation by water flow and sediment during use, which seriously affects the durability of hydraulic structures and even affects the service safety of the structures.

[0003] In my country, the research on the anti-abrasion performance of concrete mainly focuses on improving the performance of concrete itself, including improving the strength of concrete, adding fly ash, silica powder, flexible particles and special admixtures to concrete to improve its anti-abrasion performance. When the improvement of the anti-abrasion performance of concrete itself is limited, it is necessary to increase the overall anti-abrasion ability of hydraulic concrete buildings by adding a wear-resistant protective layer on its surface. The protective layer mainly includes stainless steel plates, cast stone plates, strip stone plates and protective coatings formed by brushing organic polymer anti-abrasion materials on the surface of concrete (such as epoxy resin-based anti-abrasion materials, polyurea elastomers, etc.), which are used to improve the anti-abrasion performance of hydraulic structures. These materials each have their own advantages and disadvantages. The main defects at present are: 1) limited wear resistance. The wear resistance of natural materials is only slightly improved compared to high-strength concrete; 2) weak bonding ability with the base concrete. Some resins, polyurea and other materials have good wear resistance themselves, but are difficult to coordinate with concrete and can be easily lifted off as a whole; 3) It is difficult to maintain integrity. Materials such as stone slabs and steel plates are difficult to maintain integrity and have joints, which can easily be washed away under high-speed water pressure.

[0004] In the prior art, invention publication CN 116947407A provides an abrasion-resistant mortar, wherein the mortar is prepared by mixing raw materials such as cement, water, and fine aggregate, and the mortar having chloride ion corrosion resistance and abrasion resistance is formed through the hydration reaction of cement-based cementitious materials. The invention mainly adopts the form of mortar to provide abrasion resistance, and its abrasion resistance is relatively low. Existing studies have shown that the ability of abrasion-resistant mortar to repair abrasion-resistant concrete depends on the material properties on the one hand, and on the bonding performance between the mortar and concrete on the other hand.

[0005] The existing invention patent CN 116854409A provides a preparation method for improving the anti-abrasion performance of geopolymer concrete based on nano-silicon dioxide and mixed fiber reinforcement. The raw materials include cementitious materials, aggregates, alkali activators, reinforcing materials and water. However, the dispersion effect of nanomaterials and fibers in concrete is poor in actual engineering applications, and the process cannot be guaranteed.

[0006] The existing invention patent CN 116813268A provides a wear-resistant and impact-resistant high-strength rubber concrete and its preparation method. The high-strength rubber concrete is mainly made of cement, silica fume, ultrafine cement, fly ash, coarse and fine aggregates, rubber, admixtures and water. The invention mainly obtains the most dense stacking ratio according to the material stacking density, and its performance is better than that of ordinary rubber concrete, but it is more suitable for new concrete projects.

[0007] The existing invention patent CN 116770776A provides a long-life anti-wear repair technology based on hydrophilic low-viscosity polyurethane modified interface glue TG and high thixotropic rheological modifier TV, which is characterized by first applying the hydrophilic low-viscosity polyurethane modified interface glue TG, and then pouring the strain-enhanced inorganic metal anti-wear material thereon. There are two key interface positions in the invention, one is between the polyurethane interface glue and the concrete matrix, and the other is between the polyurethane cleansing glue and the poured strain-enhanced inorganic metal anti-wear material. The improved interface bonding strength is about 4MPa, which is about 20% lower than that of the present invention. At the same time, the cost of inorganic non-metallic materials is relatively high in practical application projects, which is not conducive to large-scale repair projects.

[0008] The existing invention patent CN 116477894A provides an anti-abrasion ultra-high performance concrete and its preparation method, wherein the concrete materials mainly include high iron phase silicate cement, fly ash, silica fume, sand, steel fiber, modified rubber particles, modified graphene oxide, expansion agent, water reducer, and water. According to actual engineering research, in large-scale water conservancy projects, coarse aggregate is an important part of resisting bedload abrasion due to its high strength. The modification of rubber materials complicates the overall process test, and rubber particles and steel fibers are not easy to disperse evenly.

[0009] The existing invention patent CN 110015869A provides a method for preparing an anti-abrasion hydraulic facing block based on geopolymer, wherein an adhesive layer is provided between the geopolymer and the concrete, and the geopolymer is bonded to the surface of the concrete block by an adhesive in the form of a coating. Since the strength of the adhesive layer directly determines whether the facing is easy to fall off and be damaged, and as a prefabricated component, the construction technology and transportation are subject to certain limitations.

[0010] The existing invention CN 101759427A provides an inorganic high impact and wear resistant concrete repair material, which is mainly made of silicate minerals, volcanic ash mixture, silicon dioxide powder, sulphoaluminate minerals, fatty alcohol polyoxyethylene ether high molecular weight polymers, cellulose ether, polypropylene fibers, silicon dioxide solid particles and other raw materials, and forms a wear-resistant layer with a certain strength through chemical reaction. The invention contains many components, and the fibers in the components are not easy to disperse evenly.

[0011] The existing invention CN 114686148A provides an impact-resistant and wear-resistant material for repairing the national six surfaces of buildings with epoxy resin as a binder, quartz stone and quartz sand as raw materials, and a preparation method thereof, wherein quartz stone with the largest particle size is added to the maximum extent, thereby improving the impact and wear resistance of the material. The existing invention CN 113736402A provides a method for preparing a polymer environmentally friendly impact-resistant and anti-deterioration epoxy resin mortar, which is mainly prepared by mixing epoxy resin, surfactant additive, epoxy cyclohexyl-cage polysilsesquioxane, silane coupling agent, fumed silica, unsaturated polyester resin, unsaturated polyester resin, brominated nano-calcium, curing agent, DMP-30 accelerator, ultraviolet absorber, aramid fiber powder, flame retardant, graphene oxide nanosheets, etc. The prepared epoxy mortar has high strength, toughness and impact and wear resistance. Existing invention CN 115611554A provides a modified epoxy resin anti-abrasion repair mortar and its preparation method, which mainly includes epoxy resin, active diluent, curing agent, and asparagine polyurea prepolymer. The toughness and anti-abrasion performance of epoxy mortar are further improved mainly by the chemical reaction of epoxy groups in epoxy resin and secondary amine groups in asparagine polyurea prepolymer. Existing invention CN 112961570A provides an environmentally friendly underwater toughened epoxy resin glue and its preparation method, which also uses epoxy resin as the main raw material to provide anti-abrasion performance for the coating. Existing invention CN 104261765A provides an epoxy resin polymer mortar and production process, which is mainly formed by mixing epoxy resin slurry, active diluent, curing mixture and base material, and can improve the anti-abrasion performance of concrete. Existing invention CN 101607806A provides an anti-abrasion and anti-seepage material for concrete water-passing surface, which mainly uses epoxy resin as the main material. The existing invention CN 105366994A provides an impact-resistant epoxy resin mortar and a preparation method, which mainly uses epoxy resin to prepare impact-resistant mortar to provide concrete with impact-resistant ability. The existing invention CN107083149B provides a water tunnel concrete surface protection and shellfish-proof coating, which mainly uses a first component of epoxy resin, toughening modifier, active diluent, thixotropic agent and nano-hybrid material and a second component of benzyl alcohol diluent, nano-hybrid filler and one of polyamide curing agent, phenalkamine curing agent and modified fat curing agent.The epoxy resin material used in the above invention forms a wear-resistant layer through a polymer polymerization reaction, and has the following disadvantages: (1) Epoxy resin is relatively expensive; (2) Without the addition of other modifiers, the epoxy material has a high viscosity, which makes construction inconvenient, and the cured product is brittle; (3) Epoxy resin has a low adhesion to materials with low polarity, and these materials need to be pretreated, which complicates the construction process; (4) Epoxy resin has poor weather resistance and solidifies slowly at low temperatures. After solidification, the aromatic ether bonds therein are easily broken by sunlight. This breaking effect and the impact and abrasion effect may produce a coupling effect to accelerate the deterioration of the wear-resistant protective layer; (5) Epoxy resin modifiers such as active diluents and curing agents have varying degrees of toxicity and irritation, and are not suitable for projects directly related to ecology.

[0012] The existing invention CN 109369151A provides an inorganic composite material resistant to impact and wear for hydraulic structures and a preparation method thereof, wherein an integral inorganic composite material is prepared from aluminum nitride ceramic powder, polytetrafluoroethylene, attapulgite, acrylic rubber powder, hydroxypropyl methylcellulose, glass microspheres, slag and basalt fiber. The invention uses a room temperature reaction, and compared with the low temperature melting preparation process proposed in the present invention, the mechanical properties, wear resistance and overall performance are significantly different.

[0013] The existing invention CN 107445545 A provides a high-ductility cement-based composite material for repairing hydraulic concrete structures, which is composed of the following components by mass: 20-60 parts of cement, 0-80 parts of fly ash, 0-80 parts of ground slag, 5-10 parts of light calcium powder, 1-5 parts of nano-SiO2, 25-40 parts of fine aggregate, 20-40 parts of water, 0.1-1 parts of water reducer, and 0.5-2.5 parts of polyvinyl alcohol fiber. This method still forms a cement-based material, which is significantly different from the ceramic wear-resistant protective layer prepared by the present invention, and its anti-wear performance is weaker than that of the present invention.

[0014] The existing invention CN 104790349 A provides a hydraulic concrete structure with a ceramic plate as a protective layer, including a hydraulic concrete structure body, a plurality of expansion bolts are arranged on the hydraulic concrete structure body, a plurality of ceramic plates are arranged outside the hydraulic concrete structure body, the upper and lower ends of the ceramic plates are connected to the expansion bolts through connectors, and the ceramic plates and the hydraulic concrete structure body are bonded together by bonding mortar. The invention uses bonding mortar to bond the ceramic plates to the concrete structure, and its performance is greatly affected by the bonding mortar.

[0015] The existing invention CN 104387114 A provides a water-immune nano-polyurea hydraulic concrete repair material and a preparation method thereof. The repair material is mainly formed by a high molecular polymer reaction, which is significantly different from the low-temperature melting process proposed in the present invention. The present invention has higher impact resistance and higher hardness.

[0016] The existing invention CN 109749409A provides an aging-resistant and impact-resistant ceramic composite material specially used for hydraulic structures: firstly, a polyurethane-type epoxy resin is synthesized, and then a high-strength fiber is compounded with a graded superhard particle filler to prepare a fiber / graded superhard particle composite material, and then the polyurethane-type epoxy resin and an unmodified epoxy resin are mixed in proportion, and the fiber / graded superhard particle composite material, an active diluent, and a defoaming agent are added, stirred, and then an appropriate amount of a curing agent is added to prepare an aging-resistant and impact-resistant polyurethane-type epoxy resin / ceramic composite material. The repair material is prepared by a room temperature reaction method, and the mechanical properties and wear resistance are both low.

[0017] The existing invention CN 103420642 A provides a highly elastic abrasion-resistant mortar repair material and construction process, which is mainly characterized by the use of single-component polyurea and special sand. This is significantly different from the low-temperature melting method proposed in the present invention for preparing a ceramic protective layer. The protective layer prepared by the preparation method of the present invention has a strong bonding performance with the concrete substrate and has higher abrasion resistance and corrosion resistance.

[0018] The existing invention CN 108753100 A provides a water-based epoxy concrete repair interface agent and a preparation method thereof. The interface agent comprises component A and component B, wherein component A comprises 5% to 30% of nano-silicon dioxide emulsion, 50% to 65% of silane coupling agent, and 5% to 45% of water-based epoxy resin by mass percentage; component B comprises 30% to 50% of flexible polyetheramine and 50% to 70% of diethyltoluenediamine by mass percentage. The repair materials used in the invention are all organic polymer materials. Compared with the present invention, the present invention has higher abrasion resistance and better corrosion resistance. Summary of the invention

[0019] In order to improve the impact resistance, wear resistance and corrosion resistance of newly built hydraulic concrete buildings, as well as the repair and protection performance of hydraulic concrete buildings, and reduce the economic cost of multiple repairs of concrete structures, the present invention provides a method for preparing a hydraulic concrete low-temperature melting anti-impact and wear repair and protection layer and its repair and protection material.

[0020] As a hydraulic concrete anti-abrasion repair protective layer, when the anti-abrasion performance of the hydraulic concrete material itself reaches its limit or is damaged, from the perspective of external anti-abrasion, an anti-impact, wear-resistant and corrosion-resistant protective coating is provided on the outside of the hydraulic concrete structure damaged by impact and abrasion or on the surface of the newly formed hydraulic concrete. The protective layer is combined with the concrete into a whole through a fusion construction method, so that it has good overall performance, thereby improving the anti-impact, wear-resistant and corrosion-resistant performance of the hydraulic concrete surface.

[0021] In other fields, ceramic materials are a kind of material with excellent wear resistance and corrosion resistance, high strength, high temperature resistance, water immersion resistance, and deformation capacity close to that of concrete. If a ceramic protective layer can be made on the surface of concrete, the wear resistance of concrete can be greatly improved. The wear-resistant repair protective layer of the present invention can form an integral layer on the surface of concrete and is not easy to peel off. The present invention is a creative technical solution proposed under the guidance of this idea.

[0022] The technical solution of the present invention is: the present invention provides a preparation method and application measures for improving the anti-impact and wear repair protective layer of hydraulic concrete. The anti-impact and wear protection method of hydraulic concrete includes protective layer material components, protective layer material combination ratios, protective layer preparation process and specific construction application methods.

[0023] A hydraulic concrete low-temperature melting anti-abrasion repair and protection material, the repair and protection material is a mixture of water, potassium oxide, silicon dioxide and aluminum oxide, which is evenly covered on the concrete surface and then sintered on the concrete surface by low-temperature melting technology to form the concrete and the repair and protection material into a whole; the components in the mixture are mixed in the following mass proportions: 10-25 parts of water, 1.30-1.63 parts of potassium oxide, 4.0-4.5 parts of silicon dioxide and 1-1.2 parts of aluminum oxide.

[0024] In order to reduce the porosity of the reaction mixture material, 3 to 6 parts of mineral filler can be added to the mixture.

[0025] The mineral filler is muscovite or cordierite with a mesh size of 100 to 200.

[0026] Preferably, the components in the mixture are mixed in the following mass proportions:

[0027] 10-25 parts of water, 1.30-1.63 parts of potassium oxide, 4.0-4.5 parts of silicon dioxide, 1-1.2 parts of aluminum oxide, and 5 parts of 100-200 mesh muscovite.

[0028] Different components have different impact and wear resistance effects, which mainly depends on the content of polysilicate-silicon oxide generated by silicon, potassium and aluminum components in the components, as well as the filler composition in the mixture.

[0029] Preferably, in the mixture, the weight proportions of the substances are as follows: potassium oxide / silicon dioxide = 0.28-0.41, silicon dioxide / aluminum oxide = 3.33-4.50, water / aluminum oxide = 10-25, and potassium oxide / aluminum oxide = 1.08-1.63.

[0030] The application of the anti-abrasion repair and protection material in the repair of hydraulic concrete buildings.

[0031] The application of the anti-abrasion repair and protection material in the preparation of hydraulic concrete buildings with anti-abrasion, anti-corrosion and anti-corrosion properties. The surface of hydraulic concrete that needs to be repaired or protected is covered with the repair and protection material, and a low-temperature melting technology is used to prepare an anti-abrasion and anti-corrosion protective layer, which has good bonding performance with concrete.

[0032] A method for anti-abrasion protection construction includes covering the surface of hydraulic concrete that needs to be repaired or protected with a repair and protection material, and using low-temperature melting technology to prepare an anti-abrasion and anti-corrosion protective layer. The protective layer has good bonding performance with the concrete to form an integrated whole, thereby improving the anti-abrasion performance of the hydraulic concrete.

[0033] The low-temperature melting technology is to use a flame spray gun to melt the protective material at a low temperature, with the spray distance maintained at 50 cm to 70 cm, the temperature maintained at 85° C. to 120° C., and the time being 10 min to 30 min.

[0034] The thickness of the anti-abrasion and anti-corrosion protective layer is controlled at 1 mm to 5 mm.

[0035] The thickness of the repair and protection material covering the surface of hydraulic concrete that needs to be repaired or protected is 5 mm~8 mm.

[0036] The present invention provides an anti-impact and wear repair protective material. Further preferably, the protective material is prepared by mixing 13.5 parts of water, 1.63 parts of potassium oxide, 4.46 parts of silicon dioxide, 1.081 parts of aluminum oxide, and 5 parts of 100-200 mesh muscovite to obtain a reactive mixture.

[0037] The reactive mixture is used as a repair and protection material mixture to evenly cover the surface of the concrete material structure by 5 mm to 8 mm. The protective material slurry is directly sintered on the concrete surface using low-temperature melting technology to form a dense ceramic structure, which repairs concrete damage and improves the concrete's anti-abrasion performance.

[0038] The specific steps of the anti-abrasion protection construction method provided by the present invention are as follows:

[0039] Step 1: Prepare hydraulic concrete specimens;

[0040] Step 2: preparing geopolymer wear-resistant repair protective layer material;

[0041] Step 3: Evenly cover the concrete surface with the material prepared in step 2 to a thickness of 5 mm to 8 mm;

[0042] Step 4: Sinter the material evenly on the concrete surface to form a whole with the concrete specimen.

[0043] The step 1 is to prepare a concrete specimen as a protective matrix material of the protective material, wherein the concrete mix ratio has no additional requirements except that it meets the concrete design specification.

[0044] The step 2: preparing the wear-resistant repair and protection material, using 13.5 parts of water, 1.63 parts of potassium oxide, 4.46 parts of silicon dioxide, 1.081 parts of aluminum oxide, and 5 parts of 100-200 mesh white mica, and mixing them to obtain a reactive mixture.

[0045] Step 3: After curing the concrete for 28 days, evenly cover the concrete surface with the mixture slurry described in step 2 to ensure uniform coverage of the material.

[0046] Step 4: Use a flame spray gun, maintain the flame spray distance at 50-70 cm, maintain the temperature at 85-120° C., and sinter for 0.5-1.5 h. Ensure the constant sintering temperature and the consistency of sintering time, quickly form the concrete and the surface protection material into a whole, and have good interface bonding performance.

[0047] Principle of the invention: The present invention utilizes the copolymerization characteristics of geopolymer materials to produce a concrete wear-resistant repair protective layer with high anti-wear performance by melting. Under the operation of low-temperature melting, the mixture in step 2 can accelerate the formation of geopolymer reaction products. The molten structure in the present invention is polysilicate-silicon oxide, forming a wear-resistant repair protective layer. A highly efficient anti-wear and anti-corrosion protective surface layer is formed on the surface of hydraulic concrete in the form of external protection, which is not only suitable for the protective layer of newly built anti-wear concrete structures, but also suitable for the repair and protection construction of existing anti-wear concrete structures.

[0048] Compared with patent CN 110015869A, the concrete repair protective coating provided by the present invention can be constructed at any time on site where conditions permit. The protective method of the present invention is an integral whole with the concrete structure and has excellent bonding properties. It is chemically bonded to the concrete structure surface and can better improve the concrete's anti-abrasion and anti-corrosion properties.

[0049] Compared with CN 101759427A, the invention has relatively fewer components and is relatively easy to disperse evenly. The protective layer material is formed into a high wear-resistant layer similar to ceramics through low-temperature melting, which has significant technical improvements in wear resistance and integrity.

[0050] Compared with CN 104790349 A, the protective layer of the present invention is directly formed on the surface of hydraulic concrete, and a ceramic reaction product is formed by low-temperature melting technology, which has better bonding ability and integrity.

[0051] Compared with CN 109749409A, the construction process of the present invention is simpler, and CN 109749409A is a repair material prepared by a room temperature reaction method. Compared with the ceramic material prepared by low-temperature melting at 85-120°C proposed in the present invention, the mechanical properties and wear resistance are lower, and the reaction process is completely different.

[0052] Compared with the high-performance, high-strength anti-abrasion concrete materials in the prior art, the present invention improves the anti-abrasion and anti-cavitation performance of hydraulic concrete materials through external action. At the same time, as a repair material, the interface bonding strength between the low-temperature melting technology and the concrete when preparing the protective layer will be better than the bonding performance between ordinary concrete and old concrete, and the performance of the protective layer is better than that of cement-based cementitious materials.

[0053] Compared with the prior art which mainly uses epoxy resin to prepare impact-resistant mortar to provide concrete with impact-resistant ability, the present invention uses a mechanism of low-temperature melting to form a ceramic impact-resistant and wear-resistant protective layer, which is significantly different. The material used in the present invention has stronger impact-resistant and corrosion-resistant properties, and is green and non-toxic throughout the construction process.

[0054] The principle of the present invention is that in a normal temperature environment, inorganic mineral resin can polymerize to form a polymer. Among them, the reaction empirical formula of potassium oxide, silicon dioxide and aluminum oxide used in the present invention is:

[0055] K n [(-Si-O2) z -Al-O2-] n · ω H2O

[0056] In the formula, z is 1, 2 or 3; K is a monovalent potassium cation; n is the degree of polycondensation; ω is 2.

[0057] The molecular formula of polyaluminosilicate is:

[0058]

[0059] In the hydrates of various polyaluminosilicates, the amount of water present is equal to the solvent water plus the bonded water in the reactants. The mixture of this principle reaction is stable and still has reaction activity after long-term storage. Beneficial Effects

[0060] Compared with the existing hydraulic concrete anti-abrasion technology, the present invention has the following advantages:

[0061] The invention provides a method for preparing a hydraulic concrete anti-abrasion repair protective layer, which can significantly improve the anti-abrasion, anti-corrosion and anti-corrosion performance of concrete, improve the external anti-abrasion ability of concrete, effectively repair concrete structures damaged by abrasion, and further improve the anti-abrasion ability of concrete after the anti-abrasion performance of concrete itself is improved;

[0062] The anti-abrasion protection method provided by the present invention can significantly enhance the anti-abrasion performance of concrete and effectively reduce the erosion of water flow on concrete structures;

[0063] The material used in the anti-abrasion protection method provided by the present invention has better anti-abrasion and anti-corrosion capabilities compared with other external protection methods;

[0064] The construction method of the present invention is simple, and can be directly operated on site if conditions permit. It is directly combined with concrete to form a whole, has strong integrity, and can better protect the concrete body.

[0065] The present invention utilizes direct high-temperature sintering of materials to form a whole with concrete, and has excellent bonding performance with new concrete structures and repairing old concrete structures. DETAILED DESCRIPTION

[0066] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. The specific embodiments described here are only used to explain the technical solution of the present invention. Example 1

[0067] This embodiment provides a method for preparing a hydraulic concrete anti-abrasion repair and protection layer for use on new hydraulic concrete, which includes the preparation and application of the anti-abrasion repair and protection layer.

[0068] The implementation steps are:

[0069] Step 1: Prepare a concrete specimen as the protective base part of the protective material according to the specification requirements (there is no requirement for the mix ratio of concrete for this patent). In this embodiment, the concrete specimen is C60 concrete prepared by using ordinary Portland cement according to the mix ratio in Table 1, with a curing age of 28 days;

[0070] Step 2: preparing an anti-impact and wear repair and protection material, using 13.5 parts of water, 1.63 parts of potassium oxide, 4.46 parts of silicon dioxide, 1.081 parts of aluminum oxide, and 5 parts of 100-200 mesh white mica, and mixing them to obtain a reactive mixture;

[0071] Step 3: Evenly cover the mixture slurry obtained in step 2 on the concrete specimen by 5 mm to ensure uniform coverage of the material;

[0072] Step 4: Use a flame spray gun, keep the flame spray distance at 70 cm, keep the temperature at 90 ° C, and the sintering time is 30 min;

[0073] Step 5: After sintering, the concrete and the surface protection material form a whole with good interface bonding properties.

[0074] Table 1 Concrete mix ratio (kg / m 3 )

[0075]

[0076] The surface gloss of the cured wear-resistant repair protective layer is good and the thickness is 5 mm. The surface hardness is 740 HV when tested by a microhardness tester, and the interface bonding strength is 6 MPa when tested by a puller. The high-speed underwater steel ball method is used to test its anti-impact performance. When the speed is set to 4000 rpm and the flow rate is 40 m / s, its 28-day anti-impact strength is 6.28×10 -3 h / (kg / m 2 ), the 28-day abrasion resistance of the C60 concrete in step 1 is 3.68×10 -3 h / (kg / m 2 ), the wear-resistant repair protective layer of the present invention has a much higher abrasion resistance than the reference concrete. The wear-resistant repair protective layer of the present invention depends on the synergistic effect of the various material components described herein, is related to the interfacial bonding performance of the reference concrete described in step 1, and has nothing to do with the abrasion resistance of the reference concrete.

[0077] At present, C50 and C60 concrete are commonly used in engineering. The effect of the present invention is higher than that of C70 concrete and is at a relatively high level, with the synergistic effect of the preparation method and the proportion. Example 2

[0078] This embodiment provides a method for preparing an anti-abrasion repair and protective layer for hydraulic concrete after the concrete is damaged by abrasion, which includes the preparation and application of the anti-abrasion repair and protective layer.

[0079] The implementation steps are:

[0080] Step 1: Prepare an anti-impact and wear repair and protection material by mixing 22.88 parts of water, 1.63 parts of potassium oxide, 4.46 parts of silicon dioxide, 1.089 parts of aluminum oxide, and 6 parts of 100-200 mesh cordierite to obtain a reactive mixture.

[0081] Step 2: Evenly cover the mixture slurry obtained in step 1 with a thickness of 8 mm on the concrete surface after impact and grinding, ensuring the uniformity of material coverage and the flatness of the material surface.

[0082] Step 3: Use a flame spray gun, keep the flame spray distance at 50 cm, the temperature at 100 °C, and the sintering time at 30 min.

[0083] Step 4: After sintering, the concrete and surface protection material form a whole with good interface bonding properties.

[0084] The surface gloss of the anti-wear repair protective layer after curing is good. The surface hardness is 500 HV tested by microhardness tester, and the interface bonding strength is 5.72 MPa tested by puller. The anti-wear performance is tested by high-speed underwater steel ball method. When the speed is set to 4000 rpm and the flow rate is 40 m / s, the 28d anti-wear strength is 5.28×10 -3 h / (kg / m 2 The abrasion resistance of the abrasion-resistant repair protective layer of the present invention depends on the synergistic effect of the various material components described herein, and has nothing to do with the abrasion resistance of the reference concrete. Example 3

[0085] The present embodiment provides a method for preparing a hydraulic concrete anti-abrasion repair protective layer, which includes the effects of material component differences of the anti-abrasion repair protective layer and the application of the protective layer.

[0086] The implementation steps are:

[0087] Step 1: Prepare hydraulic abrasion-resistant concrete specimens according to the specification requirements and cure for 28 days;

[0088] Step 2: Prepare anti-impact and wear repair and protection materials.

[0089] Component 1:

[0090] 13.5 parts of water, 1.31 parts of potassium oxide, 4.40 parts of silicon dioxide, and 1.01 parts of aluminum oxide were mixed to obtain a reactive mixture.

[0091] Component 2:

[0092] 13.5 parts of water, 1.31 parts of potassium oxide, 4.40 parts of silicon dioxide, 1.01 parts of aluminum oxide, and 3 parts of 100-200 mesh muscovite were mixed to obtain a reactive mixture.

[0093] Component three:

[0094] 23.50 mol of water, 1.63 parts of potassium oxide, 4.50 parts of silicon dioxide, 1.081 parts of aluminum oxide, and 6 parts of 100-200 mesh cordierite were mixed to obtain a reactive mixture.

[0095] Control group 1: 13.5 parts of water, 1.31 parts of potassium oxide, 1.40 parts of silicon dioxide, and 1.38 parts of aluminum oxide were mixed to obtain a reactive mixture, wherein potassium oxide / silicon dioxide=0.936, silicon dioxide / aluminum oxide=1.014, water / aluminum oxide=9.783, potassium oxide / aluminum oxide=0.949, and the component ratios are not within the scope of the present invention.

[0096] Step 3: Evenly cover the mixture slurries 1, 2, 3 and control group 1 obtained in step 2 on the concrete specimens by 5 mm to ensure uniform coverage of the material.

[0097] Step 4: The preparation methods of the three mixtures are as follows: the mixture slurry of component 1 is prepared by a flame spray gun, the flame spray distance is maintained at 70 cm, the temperature is maintained at 90°C, and the sintering time is 30 min; the mixture slurry of component 2 is prepared by a flame spray gun, the flame spray distance is maintained at 50 cm, the temperature is maintained at 85°C, and the sintering time is 15 min; the mixture slurry of component 3 is prepared by a flame spray gun, the flame spray distance is maintained at 60 cm, the temperature is maintained at 100°C, and the sintering time is 20 min; the mixture slurry of control group 1 is prepared by a flame spray gun, the flame spray distance is maintained at 70 cm, the temperature is maintained at 90°C, and the sintering time is 30 min;

[0098] Step 5: After sintering, the concrete and the surface protection material form a whole with good interface bonding properties.

[0099] The surface gloss of the anti-wear repair protective layer after curing is good. The surface parameters of the anti-wear repair protective layer after curing are shown in Table 2.

[0100] Control group 2: 13.5 parts of water, 1.31 parts of potassium oxide, 4.40 parts of silicon dioxide, 1.01 parts of aluminum oxide, and 3 parts of 100-200 mesh muscovite were mixed to obtain a reactive mixture. The mixture was covered on the concrete specimen by 5 mm to ensure uniform coverage of the material. The room temperature curing method was adopted and the curing was carried out for 7 days. The surface parameters of the anti-wear repair protective layer after curing are shown in Table 2.

[0101] Table 2 Performance of impact-resistant and wear-resistant protective layers of different components in Example 3

[0102] Mix ratio Surface hardness / HV Interface bonding strength / MPa <![CDATA[Abrasion and impact resistance strength / ×10 -3 h / (kg / m 2 )]]> Component 1 614 5.0 5.02 Component 2 650 5.8 5.67 Component Three 702 6.4 6.78 Control group 1 578 4.6 4.89 Control group 2 428 3.7 3.48

[0103] It can be seen from Table 2 that different components have different impact resistance and wear resistance, which mainly depends on the content of polysilicate-silicon oxide generated by silicon, potassium and aluminum components in the components, as well as the filler composition in the mixture. The addition of fillers can improve the impact resistance and wear resistance. The protective material adopts the content of material components as the most preferred mix ratio.

Claims

1. A hydraulic concrete low-temperature melting anti-abrasion repair and protection material, characterized in that: The repair and protection material is a mixture of water, potassium oxide, silicon dioxide and aluminum oxide, which is evenly covered on the surface of concrete, and then sintered on the surface of concrete by low-temperature melting technology to form a sintered anti-impact and wear repair and protection layer, at which time the concrete and the repair and protection material form a whole; the components in the mixture are mixed in the following mass proportions: 10-25 parts of water, 1.30-1.63 parts of potassium oxide, 4.0-4.5 parts of silicon dioxide, 1-1.2 parts of aluminum oxide, and 3-6 parts of mineral fillers, and the mineral fillers are 100-200 mesh white mica or cordierite; The low-temperature melting technology is to use a flame spray gun to melt the protective material at a low temperature, with the spray distance maintained at 50 cm to 70 cm, the temperature maintained at 85° C. to 120° C., and the time being 10 min to 30 min.

2. The hydraulic concrete low-temperature melting anti-abrasion repair and protection material according to claim 1 is characterized in that: The components in the mixture are mixed in the following mass proportions: 10-25 parts of water, 1.3-1.52 parts of potassium oxide, 4.0-4.2 parts of silicon dioxide, 1 part of aluminum oxide, and 3-6 parts of 100-200 mesh muscovite or cordierite as mineral filler.

3. The hydraulic concrete low-temperature melting anti-abrasion repair and protection material according to claim 1 is characterized in that: The weight proportions of the various substances in the mixture are: potassium oxide / silicon dioxide = 0.28~0.41, silicon dioxide / aluminum oxide = 3.33~4.50, water / aluminum oxide = 10~25, potassium oxide / aluminum oxide = 1.08~1.

63.

4. Use of the hydraulic concrete low-temperature melting anti-abrasion repair and protection material according to any one of claims 1 to 3 in the repair of hydraulic concrete buildings.

5. The use according to claim 4, characterized in that: The surface of hydraulic concrete that needs to be repaired or protected is covered with repair and protection materials, and a low-temperature melting technology is used to prepare an anti-abrasion and anti-corrosion protective layer. The protective layer has good bonding properties with the concrete, forming an integrated whole, thereby improving the anti-abrasion performance of the hydraulic concrete.

6. The use according to claim 5, characterized in that: The low-temperature melting technology is to use a flame spray gun to melt the protective material at a low temperature, with the spray distance maintained at 50 cm to 70 cm, the temperature maintained at 85° C. to 120° C., and the time being 10 min to 30 min.

7. The use according to claim 5, characterized in that: The thickness of the anti-abrasion and anti-corrosion protective layer is controlled at 1 mm to 5 mm.

8. The use according to claim 5, characterized in that: The thickness of the repair and protection material covering the surface of hydraulic concrete that needs to be repaired or protected is 5 mm~8 mm.