Solar Cells

By growing vertically arranged silicon dioxide carbon nanotube array structure on solar cells, the anti-reflection film layer is formed, which solves the problem of high reflectivity of silicon-based solar cells, improves light absorption efficiency, simplifies the preparation process, and reduces costs .

CN117577696BActive Publication Date: 2024-11-12TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311619720.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-11-12
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

The reflectivity of existing silicon-based solar cells is high, resulting in low optical absorption efficiency, and the preparation process of the anti-reflection structure on the pyramid surface is complex and costly.

Method used

Using an anti-reflective film layer composed of silica carbon nanotubes, an array structure is formed by growing vertically arranged silica carbon nanotubes on the battery body to reduce light reflection, and through specific template agent and solvent ratios and preparation Methods to improve the yield and uniformity of nanotubes.

Benefits of technology

It effectively reduces the reflectivity of the solar cell, improves the solar energy absorption efficiency of the specific surface area, improves the conversion efficiency of the solar cell, simplifies the preparation process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117577696B_ABST
    Figure CN117577696B_ABST
Patent Text Reader

Abstract

The present invention discloses a solar cell. The solar cell includes a cell body and an anti-reflection film layer. The anti-reflection film layer is located on the light-receiving surface of the cell body. The anti-reflection film layer is composed of a plurality of silicon dioxide carbon nanotubes. The silicon dioxide carbon nanotubes are perpendicular to the light-receiving surface of the cell body. The solar cell of the present application can reduce the reflectivity of the solar cell, increase the specific surface area, absorb more solar energy per unit area, and improve the conversion efficiency of the solar cell. The silicon dioxide carbon nanotubes of the present application can achieve the effects of high yield, large aspect ratio, and uniform size during preparation. The anti-reflection film layer formed by the silicon dioxide nanotubes can reduce the reflection of sunlight, increase the absorption of sunlight, and improve the conversion efficiency of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic technology, and in particular to a solar cell. Background Art

[0002] Silicon-based solar cells dominate the world photovoltaic market due to their abundant raw material reserves, mature production technology, and high photoelectric conversion efficiency. Since the reflectivity of untreated cells is close to 40%, if they are not modified, it will seriously affect optical absorption. In commercial applications, micron-scale pyramids are usually used as surface anti-reflection structures. This surface anti-reflection structure requires suppression of light reflection, but the effect is not ideal. In addition, the preparation process of existing pyramid surface anti-reflection structures is complex and costly. Summary of the invention

[0003] Based on this, it is necessary to provide a solar cell. The solar cell of the present invention can reduce the reflectivity of the solar cell, increase the specific surface area, absorb more solar energy per unit area, and improve the conversion efficiency of the solar cell.

[0004] An embodiment of the present application provides a solar cell.

[0005] A solar cell comprises a cell body and an anti-reflection film layer, wherein the anti-reflection film layer is located on the light-receiving surface of the cell body and is composed of a plurality of silicon dioxide carbon nanotubes, and the silicon dioxide carbon nanotubes are perpendicular to the light-receiving surface of the cell body.

[0006] In some embodiments, the plurality of silicon dioxide carbon nanotubes are in an array structure.

[0007] In some embodiments, the inner diameter of a single silicon dioxide carbon nanotube is 20 nm to 40 nm.

[0008] In some embodiments, the length of the silicon dioxide carbon nanotubes is 130 nm to 170 nm, so that the thickness of the anti-reflection film layer is 130 nm to 170 nm.

[0009] In some embodiments, the method for preparing the anti-reflection film layer comprises the following steps:

[0010] Adding a preset amount of template into a preset amount of solvent, and sonicating until completely dissolved;

[0011] Adding an ammonia solution at room temperature, inserting the battery body under stirring, adding tetraethoxysilane, and standing to allow silicon dioxide carbon nanotubes to grow on the battery body;

[0012] After a predetermined time, the battery body is taken out, cleaned and dried to obtain the anti-reflection film layer.

[0013] In some embodiments, the template is D,L-tartaric acid.

[0014] In some embodiments, the solvent is ethanol.

[0015] In some embodiments, the mass ratio of the template to the solvent is 1:(10-75).

[0016] In some embodiments, the solar cell further comprises a passivation film layer, wherein the passivation film layer is stacked on the anti-reflection film layer, and the passivation film layer is located on a surface of the anti-reflection film layer away from the solar cell body.

[0017] In some of the embodiments, the battery body includes any one of a REPC battery, a BSF battery, a SHJ battery, a TOPCon battery and an IBC battery structure.

[0018] The above solar cell can reduce the reflectivity of the solar cell, increase the specific surface area, absorb more solar energy per unit area, and improve the conversion efficiency of the solar cell. The silicon dioxide carbon nanotubes of the present application can achieve the effects of high yield, large aspect ratio, and uniform size during preparation. The anti-reflection film layer formed by the silicon dioxide nanotubes can reduce the reflection of sunlight, increase the absorption of sunlight, and improve the conversion efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0020] In order to more completely understand the present application and its beneficial effects, the following description will be given in conjunction with the accompanying drawings. In the following description, the same reference numerals represent the same parts.

[0021] Figure 1 A schematic diagram of a solar cell according to an embodiment of the present invention;

[0022] Figure 2 This is a light reflection circuit diagram of silicon dioxide carbon nanotubes in a solar cell according to an embodiment of the present invention.

[0023] Description of Reference Numerals

[0024] 10. Solar cell; 100. Cell body; 200. Anti-reflection film layer; 201. Silicon dioxide carbon nanotubes; 300. Passivation layer. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0026] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0027] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0028] In the description of the present invention, "several" means more than one, "many" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0029] In the present invention, unless otherwise stated, the sum of the parts of each component in the composition can be 100 parts by weight. Unless otherwise specified, the basis of the percentages (including weight percentages) of the present invention is the total weight of the composition. In addition, "wt%" herein means mass percentage, and "at%" means atomic percentage.

[0030] In this article, unless otherwise stated, each reaction step may be carried out in the order described herein or may not be carried out in the order described herein. For example, other steps may be included between each reaction step, and the order of the reaction steps may also be appropriately swapped. This can be determined by the technician based on common knowledge and experience. Preferably, the reaction method herein is carried out sequentially.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0032] The embodiment of the present application provides a solar cell 10 to solve the problem that in the conventional technology, the solar cell 10 uses a pyramid as a surface anti-reflection structure, such a surface anti-reflection structure needs to suppress light reflection but the effect is not ideal, and the preparation process of the existing pyramid surface anti-reflection structure is complicated and the cost is high. The solar cell 10 will be described below in conjunction with the accompanying drawings.

[0033] The solar cell 10 provided in the embodiment of the present application is exemplary, see Figure 1 As shown, Figure 1 The solar cell 10 of the present application can reduce the reflectivity of the solar cell 10, increase the specific surface area, absorb more solar energy per unit area, and improve the conversion efficiency of the solar cell 10.

[0034] In order to more clearly illustrate the structure of the solar cell 10 , the solar cell 10 will be introduced below with reference to the accompanying drawings.

[0035] For example, see Figure 1 As shown, Figure 1 A schematic diagram of the structure of a solar cell 10 provided in an embodiment of the present application. A solar cell 10 includes a cell body 100 and an anti-reflection film layer 200. The anti-reflection film layer 200 is located on the light-receiving surface of the cell body 100. The anti-reflection film layer 200 is composed of a plurality of silicon dioxide carbon nanotubes 201. The silicon dioxide carbon nanotubes 201 are perpendicular to the light-receiving surface of the cell body 100. Figure 2 As shown, Figure 2 FIG. 1 is a light reflection circuit diagram of the silicon dioxide carbon nanotubes 201 in the solar cell 10 according to an embodiment of the present invention.

[0036] In some embodiments, the plurality of silicon dioxide carbon nanotubes 201 are in an array structure.

[0037] In some of the embodiments, the inner diameter of a single silicon dioxide carbon nanotube 201 is 20 nm to 40 nm. For example, in one specific example, the inner diameter of a single silicon dioxide carbon nanotube 201 is 20 nm. In another specific example, the inner diameter of a single silicon dioxide carbon nanotube 201 is 40 nm. It is not difficult to understand that in other specific examples, the inner diameter of a single silicon dioxide carbon nanotube 201 can also be 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm or other values.

[0038] In some of the embodiments, the length of the silicon dioxide carbon nanotube 201 is 130nm to 170nm, so that the thickness of the anti-reflection film layer 200 is 130nm to 170nm. For example, in one specific example, the length of the silicon dioxide carbon nanotube 201 is 130nm. In another specific example, the length of the silicon dioxide carbon nanotube 201 is 170nm. It is not difficult to understand that in other specific examples, the length of the single silicon dioxide carbon nanotube 201 can also be 132nm, 135nm, 138nm, 140nm, 143nm, 145nm, 146nm, 147nm, 150nm, 151nm, 153nm, 155nm, 158nm, 160nm, 162nm, 165nm, 167nm, 169nm or other values.

[0039] In some embodiments, the method for preparing the anti-reflection film layer 200 includes the following steps:

[0040] (1) Add a preset amount of template into a preset amount of solvent and sonicate until completely dissolved.

[0041] (2) Adding an ammonia solution at room temperature, inserting the battery body 100 under stirring, and adding tetraethoxysilane, and letting it stand, so that the silicon dioxide carbon nanotubes 201 grow on the battery body 100.

[0042] (3) After a predetermined period of time, the battery body 100 is taken out, cleaned, and dried to obtain the anti-reflection film layer 200.

[0043] In some embodiments, the template is D,L-tartaric acid.

[0044] In some embodiments, the solvent is ethanol.

[0045] In some of the embodiments, the mass ratio of the template to the solvent is 1: (10-75), preferably, the mass ratio of the template to the solvent is 1: (20-50), and more preferably, the mass ratio of the template to the solvent is 1: (30-40). In other words, the mass ratio of D, L-tartaric acid to ethanol is 1: (10-75). For example, in one specific example, the mass ratio of the template to the solvent is 1: 10. In another specific example, the mass ratio of the template to the solvent is 1: 75. It is not difficult to understand that in other specific examples, the mass ratio of the template to the solvent can also be 1: 15, 1: 20, 1: 25, 1: 30, 1: 35, 1: 40, 1: 45, 1: 50, 1: 55, 1: 60, 1: 65, 1: 70 or other ratios.

[0046] In some embodiments, the standing time is 20 min to 200 min.

[0047] For example, in some embodiments, the method for preparing the anti-reflection film layer 200 includes the following steps:

[0048] (1) Add a preset amount of template D,L-tartaric acid to a preset amount of solvent ethanol and sonicate until completely dissolved.

[0049] (2) Ammonia solution is added at room temperature of 25° C., and the battery body 100 is inserted under stirring. Tetraethoxysilane is added and the battery body is left to stand for 60 minutes, so that silicon dioxide carbon nanotubes 201 grow on the battery body 100 .

[0050] (3) After a predetermined period of time, the battery body 100 is taken out, cleaned, and dried to obtain the anti-reflection film layer 200.

[0051] In some embodiments, the solar cell 10 further includes a passivation film layer. The passivation film layer is stacked on the anti-reflection film layer 200. The passivation film layer is located on the surface of the anti-reflection film layer 200 away from the solar cell body 100.

[0052] In some of the embodiments, the passivation film layer may be a silicon nitride layer.

[0053] In some of the embodiments, the battery body 100 includes any one of a REPC battery, a BSF battery, a SHJ battery, a TOPCon battery, and an IBC battery structure.

[0054] Example 1

[0055] This embodiment provides a solar cell 10 .

[0056] The solar cell 10 of this embodiment includes a cell body 100 and an anti-reflection film layer 200 , wherein the solar cell 10 is a REPC cell structure.

[0057] The anti-reflection film layer 200 is located on the light-receiving surface of the battery body 100. The anti-reflection film layer 200 is composed of a plurality of silicon dioxide carbon nanotubes 201. The silicon dioxide carbon nanotubes 201 are perpendicular to the light-receiving surface of the battery body 100. A passivation film layer is also provided on the surface of the anti-reflection film layer 200 away from the battery body 100.

[0058] The plurality of silicon dioxide carbon nanotubes 201 on the anti-reflection film layer 200 are in an array structure, and the inner diameter of a single silicon dioxide carbon nanotube 201 is 20 nm. The length of the silicon dioxide carbon nanotube 201 is 130 nm, so that the thickness of the anti-reflection film layer 200 is 130 nm.

[0059] The method for preparing the anti-reflection film layer 200 comprises the following steps:

[0060] (1) Add 1 part of the template D,L-tartaric acid to 75 parts of the solvent ethanol and sonicate until it is completely dissolved.

[0061] (2) Ammonia solution is added at room temperature of 25° C., and the battery body 100 is inserted under stirring. Tetraethoxysilane is added and the battery body is left to stand for 60 minutes, so that silicon dioxide carbon nanotubes 201 grow on the battery body 100 .

[0062] (3) After the battery body 100 is taken out, it is cleaned and dried to obtain the anti-reflection film layer 200.

[0063] Example 2

[0064] This embodiment provides a solar cell 10 .

[0065] The solar cell 10 of this embodiment includes a cell body 100 and an anti-reflection film layer 200 , wherein the solar cell 10 is an IBC cell structure.

[0066] The anti-reflection film layer 200 is located on the light-receiving surface of the battery body 100. The anti-reflection film layer 200 is composed of a plurality of silicon dioxide carbon nanotubes 201. The silicon dioxide carbon nanotubes 201 are perpendicular to the light-receiving surface of the battery body 100. A passivation film layer is also provided on the surface of the anti-reflection film layer 200 away from the battery body 100.

[0067] The plurality of silicon dioxide carbon nanotubes 201 on the anti-reflection film layer 200 are in an array structure, and the inner diameter of a single silicon dioxide carbon nanotube 201 is 40 nm. The length of the silicon dioxide carbon nanotube 201 is 170 nm, so that the thickness of the anti-reflection film layer 200 is 170 nm.

[0068] The method for preparing the anti-reflection film layer 200 comprises the following steps:

[0069] (1) Add 2 parts of the template D,L-tartaric acid to 50 parts of the solvent ethanol and sonicate until completely dissolved.

[0070] (2) Ammonia solution is added at room temperature of 25° C., and the battery body 100 is inserted under stirring. Tetraethoxysilane is added and the battery body is left to stand for 60 minutes, so that silicon dioxide carbon nanotubes 201 grow on the battery body 100 .

[0071] (3) After the battery body 100 is taken out, it is cleaned and dried to obtain the anti-reflection film layer 200.

[0072] Example 3

[0073] This embodiment provides a solar cell 10 .

[0074] The solar cell 10 of this embodiment includes a cell body 100 and an anti-reflection film layer 200 , wherein the solar cell 10 is a TOPCon cell structure.

[0075] The anti-reflection film layer 200 is located on the light-receiving surface of the battery body 100. The anti-reflection film layer 200 is composed of a plurality of silicon dioxide carbon nanotubes 201. The silicon dioxide carbon nanotubes 201 are perpendicular to the light-receiving surface of the battery body 100. A passivation film layer is also provided on the surface of the anti-reflection film layer 200 away from the battery body 100.

[0076] The plurality of silicon dioxide carbon nanotubes 201 on the anti-reflection film layer 200 are in an array structure, and the inner diameter of a single silicon dioxide carbon nanotube 201 is 30 nm. The length of the silicon dioxide carbon nanotube 201 is 150 nm, so that the thickness of the anti-reflection film layer 200 is 150 nm.

[0077] The method for preparing the anti-reflection film layer 200 comprises the following steps:

[0078] (1) Add 0.5 parts of the template agent D,L-tartaric acid to 30 parts of the solvent ethanol and sonicate until it is completely dissolved.

[0079] (2) Ammonia solution is added at room temperature of 25° C., and the battery body 100 is inserted under stirring. Tetraethoxysilane is added and the battery body is left to stand for 90 minutes, so that silicon dioxide carbon nanotubes 201 grow on the battery body 100 .

[0080] (3) After the battery body 100 is taken out, it is cleaned and dried to obtain the anti-reflection film layer 200.

[0081] Comparative Example 1

[0082] This comparative example 1 provides a solar cell.

[0083] The solar cell of this comparative example 1 is basically the same in structure as the solar cell of Example 1, except that the anti-reflection film layer in comparative example 1 is an ultra-thin silicon nitride covering layer.

[0084] Specifically, the solar cell in comparative example 1 includes a cell body, an anti-reflection film layer, and a passivation film layer, wherein the solar cell is a REPC cell structure. The anti-reflection film layer is located on the light-receiving surface of the cell body. The anti-reflection film layer is an ultra-thin silicon nitride covering layer. The thickness of the anti-reflection film layer is 130 nm.

[0085] Comparative Example 2

[0086] This comparative example 2 provides a solar cell.

[0087] The solar cell of Comparative Example 2 is basically the same in structure as the solar cell of Example 2, except that the anti-reflection film layer in Comparative Example 2 is an ultra-thin silicon nitride covering layer.

[0088] Specifically, the solar cell in comparative example 1 includes a cell body, an anti-reflection film layer, and a passivation film layer, wherein the solar cell is an IBC cell structure. The anti-reflection film layer is located on the light-receiving surface of the cell body. The anti-reflection film layer is an ultra-thin silicon nitride covering layer. The thickness of the anti-reflection film layer is 170 nm.

[0089] Comparative Example 3

[0090] This comparative example 3 provides a solar cell.

[0091] The solar cell of comparative example 3 is basically the same in structure as the solar cell of embodiment 3, except that the anti-reflection film layer in comparative example 3 is an ultra-thin silicon nitride covering layer.

[0092] Specifically, the solar cell in comparative example 1 includes a cell body, an anti-reflection film layer, and a passivation film layer, wherein the solar cell is a TOPCon cell structure. The anti-reflection film layer is located on the light-receiving surface of the cell body. The anti-reflection film layer is an ultra-thin silicon nitride covering layer. The thickness of the anti-reflection film layer is 150 nm.

[0093] Comparative Example 4

[0094] This comparative example 4 provides a solar cell.

[0095] The solar cell of Comparative Example 4 has a substantially similar structure to that of the solar cell of Example 1, except that the thickness of the anti-reflection film layer in Comparative Example 4 is 250 nm.

[0096] Specifically, the anti-reflection film layer is located on the light-receiving surface of the battery body. The anti-reflection film layer is composed of a plurality of silicon dioxide carbon nanotubes. The silicon dioxide carbon nanotubes are perpendicular to the light-receiving surface of the battery body. A passivation film layer is also provided on the surface of the anti-reflection film layer away from the battery body.

[0097] The plurality of silicon dioxide carbon nanotubes on the anti-reflection film layer are in an array structure, and the inner diameter of a single silicon dioxide carbon nanotube is 20 nm. The length of the silicon dioxide carbon nanotube is 250 nm, so that the thickness of the anti-reflection film layer is 250 nm.

[0098] The method for preparing the anti-reflection film layer comprises the following steps:

[0099] (1) Add 3 parts of the template D,L-tartaric acid to 45 parts of the solvent ethanol and sonicate until completely dissolved.

[0100] (2) Adding an ammonia solution at room temperature of 25° C., inserting the battery body under stirring, and adding tetraethoxysilane, the battery body was left standing for 60 minutes to allow silicon dioxide carbon nanotubes to grow on the battery body.

[0101] (3) After taking out the battery body, cleaning and drying it, an anti-reflection film layer is obtained.

[0102] Comparative Example 5

[0103] This comparative example 5 provides a solar cell.

[0104] The solar cell of Comparative Example 5 is basically the same in structure as the solar cell of Example 1, except that the thickness of the anti-reflection film layer in Comparative Example 5 is 90 nm.

[0105] Specifically, the anti-reflection film layer is located on the light-receiving surface of the battery body. The anti-reflection film layer is composed of a plurality of silicon dioxide carbon nanotubes. The silicon dioxide carbon nanotubes are perpendicular to the light-receiving surface of the battery body. A passivation film layer is also provided on the surface of the anti-reflection film layer away from the battery body.

[0106] The plurality of silicon dioxide carbon nanotubes on the anti-reflection film layer are in an array structure, and the inner diameter of a single silicon dioxide carbon nanotube is 20 nm. The length of the silicon dioxide carbon nanotube is 90 nm, so that the thickness of the anti-reflection film layer is 90 nm.

[0107] The method for preparing the anti-reflection film layer comprises the following steps:

[0108] (1) Add 1.5 parts of the template D,L-tartaric acid to 60 parts of the solvent ethanol and sonicate until it is completely dissolved.

[0109] (2) Adding an ammonia solution at room temperature of 25° C., inserting the battery body under stirring, and adding tetraethoxysilane, the battery body was left standing for 60 minutes to allow silicon dioxide carbon nanotubes to grow on the battery body.

[0110] (3) After taking out the battery body, cleaning and drying it, an anti-reflection film layer is obtained.

[0111] The performance tests were conducted on the solar cells 10 in Examples 1 to 3 and Comparative Examples 1 to 5. The test results are shown in Table 1.

[0112] Table 1

[0113] Reflectivity Transformation efficiency Example 1 0.5% 22.9% Example 2 0.9% 22.4% Example 3 1.2% 22.3% Comparative Example 1 6.1% 21.6% Comparative Example 2 6.6% 21.5% Comparative Example 3 6.9% 21.4% Comparative Example 4 7% 20.9% Comparative Example 5 7.5% 20.7%

[0114] As can be seen from Table 1, by comparing Example 1 with Comparative Example 1, comparing Example 2 with Comparative Example 2, and comparing Example 3 with Comparative Example 3, it can be seen that the multiple silicon dioxide carbon nanotubes on the anti-reflection film layer 200 of the present application can reduce light reflectivity, increase the specific surface area, absorb more solar energy per unit area, and improve the conversion efficiency of the solar cell 10. By comparing Comparative Examples 4 and 5 with Example 1, it can be seen that the length of the silicon dioxide carbon nanotubes in the present application is 130nm~170nm, so that the thickness of the anti-reflection film layer 200 is 130nm~170nm, which can effectively reduce the reflectivity of the solar cell 10. When the length of the silicon dioxide carbon nanotubes is less than 130nm, for example, the length of the silicon dioxide carbon nanotubes in Comparative Example 5 is 90nm, the reflectivity of the solar cell 10 is not as good as that of Example 1. When the length of the silicon dioxide carbon nanotubes is greater than 170nm, for example, the length of the silicon dioxide carbon nanotubes in Comparative Example 4 is 250nm, the reflectivity of the solar cell 10 is not as good as that of Example 1, and the material cost will also increase significantly. Therefore, it can be seen that the length of the silicon dioxide carbon nanotubes in the present application is 130nm~170nm, which can save materials and reduce the reflectivity of the solar cell 10.

[0115] In summary, the solar cell 10 of the present application can reduce the reflectivity of the solar cell 10, increase the specific surface area, absorb more solar energy per unit area, and improve the conversion efficiency of the solar cell 10. The silicon dioxide carbon nanotubes of the present application can achieve the effects of high yield, large aspect ratio, and uniform size during preparation, and the anti-reflection film layer 200 formed by the silicon dioxide nanotubes can reduce the reflection of sunlight, increase the absorption of sunlight, and improve the conversion efficiency of the solar cell 10.

[0116] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0117] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0118] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A solar cell, characterized in that: It includes a battery body and an anti-reflection film layer, wherein the anti-reflection film layer is located on the light-receiving surface of the battery body, and the anti-reflection film layer is composed of a plurality of silicon dioxide carbon nanotubes, and the silicon dioxide carbon nanotubes are perpendicular to the light-receiving surface of the battery body; The inner diameter of a single silicon dioxide carbon nanotube is 20 nm to 40 nm, and the length of the silicon dioxide carbon nanotube is 130 nm to 170 nm, so that the thickness of the anti-reflection film layer is 130 nm to 170 nm.

2. The solar cell according to claim 1, characterized in that: The plurality of silicon dioxide carbon nanotubes are in an array structure.

3. The solar cell according to claim 1, characterized in that: The method for preparing the anti-reflection film layer comprises the following steps: Adding a preset amount of template into a preset amount of solvent, and sonicating until completely dissolved; Adding an ammonia solution at room temperature, inserting the battery body under stirring, adding tetraethoxysilane, and standing to allow silicon dioxide carbon nanotubes to grow on the battery body; After a predetermined time, the battery body is taken out, cleaned and dried to obtain the anti-reflection film layer.

4. The solar cell according to claim 3, characterized in that: The template is D,L-tartaric acid.

5. The solar cell according to claim 3, characterized in that: The solvent is ethanol.

6. The solar cell according to claim 3, characterized in that: The mass ratio of the template to the solvent is 1:(10-75).

7. The solar cell according to any one of claims 1 to 6, characterized in that: The solar cell further comprises a passivation film layer, which is stacked on the anti-reflection film layer and is located on a surface of the anti-reflection film layer away from the cell body.

8. The solar cell according to any one of claims 1 to 6, characterized in that: The battery body includes any one of a REPC battery, a BSF battery, a SHJ battery, a TOPCon battery and an IBC battery structure.