A kind of hydrophilic polyurethane filler and preparation method thereof

By using a simple preparation method of combining polyether polyol and MDI with konjac glucomannan-acrylic acid graft copolymer, the problem of poor hydrophilicity of polyurethane sponges is solved, and efficient wastewater treatment effect is achieved, providing an operation Simple and low-cost hydrophilic polyurethane filler.

CN117586474BActive Publication Date: 2024-11-19NORTH CHINA ELECTRIC POWER UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311562940.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2024-11-19
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

The existing polyurethane sponges have poor hydrophilicity, which affects their biological reaction efficiency in wastewater treatment, and the traditional modification methods are costly or have limited effects.

Method used

Polyether polyol and MDI as the main raw materials, konjac glucomannan-acrylic acid graft copolymer and additives were added, and polyurethane fillers with good hydrophilicity were prepared by simple one-step foaming method to improve their hydrophilic properties and mounts. Film effect.

Benefits of technology

The preparation of hydrophilic polyurethane filler with simple operation and low cost is achieved, which significantly improves its hydrophilic effect and film hanging performance, and enhances the biological reaction efficiency in wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117586474B_ABST
    Figure CN117586474B_ABST
Patent Text Reader

Abstract

The invention discloses a hydrophilic polyurethane filler and a preparation method thereof. The preparation method comprises: weighing polyether polyol, an amine catalyst, dibutyltin dilaurate, an organosilicon foam stabilizer, water, dichloromethane, a hydrophilic agent, a pore opening agent, and a konjac glucomannan-acrylic acid graft copolymer in sequence in a container, stirring evenly, standing, then adding the weighed diphenylmethane diisocyanate into the container, stirring for 5-15 seconds, and then pouring into a foaming box for free foaming, and after the foaming stops, placing in an oven to continue foaming for 60 minutes, and placing for 24 hours after the foaming stops, so as to obtain the hydrophilic polyurethane filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, and more particularly to a hydrophilic polyurethane filler and a preparation method thereof. Background Art

[0002] At present, the conventional methods used in sewage treatment in my country include physical methods, chemical methods and biological methods. Among them, the physical method has low equipment cost and is easy to operate, but the treatment effect is poor. Although the treatment effect of chemical treatment is better than that of physical treatment, the cost is relatively high. Compared with traditional physical and chemical methods, the biological method based on microbial remediation has the advantages of low cost, short time consumption, not easy to bring in secondary pollution, and no destruction of ecological balance, and has attracted more and more attention from scholars. The biological method uses screened and cultured microorganisms to convert toxic and harmful pollutants into non-toxic and harmless substances through microbial degradation or biotransformation, and has been widely used in sewage treatment.

[0003] Immobilized microbial technology is a microbial treatment technology that has been developed since the 1960s. Fixing free bacteria on fillers can reduce the loss rate of microorganisms and increase the concentration of microorganisms (especially microorganisms with special functions) in bioreactors. Fillers can provide a place for microorganisms to attach and grow. Their properties such as material, surface roughness, and specific surface area directly affect the speed of biofilm formation and the amount of microorganisms, thereby affecting the effect of biological sewage treatment. Polyurethane foam (PUF) carrier is an ideal growth medium with high porosity and high specific surface area. It can be used to fix microorganisms and has the characteristics of low price, easy installation, long service life, and not easy to clog. In view of this, PUF is widely used in the field of sewage treatment.

[0004] However, most of the structural units of common polyurethane sponges on the market are hydrophobic segments and groups, so the hydrophilicity is relatively poor. In order to improve the hydrophilicity of polyurethane, water-absorbing substances can be added to the formula or hydrophilic groups or segments can be introduced into the polyurethane molecular chain. For example, Zheng Kai et al. used chemical oxidation and acrylic acid grafting technology to hydrophilize polyurethane foam (PUF) to enhance the hydrophilicity of PUF, increase its real specific surface area, reduce the surface contact angle, and effectively improve its hydrophilicity. Summary of the invention

[0005] In view of this, the present invention provides a hydrophilic polyurethane filler and a preparation method thereof, which uses polyether polyol and MDI as main raw materials, and adds konjac glucomannan-acrylic acid graft copolymer and various additives, so as to prepare a polyurethane filler with good hydrophilicity and fast biofilm effect by a simple one-step foaming method.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A hydrophilic polyurethane filler comprises the following components in parts by weight:

[0008] 95-105 parts of polyether polyol, 55-65 parts of MDI (diphenylmethane diisocyanate), 25-35 parts of hydrophilic agent, 10-20 parts of pore opener, 2-4 parts of konjac glucomannan-acrylic acid graft copolymer, 1-2 parts of dibutyltin dilaurate, 1-2 parts of silicone foam stabilizer, 1-2 parts of water, 0.5-1 parts of dichloromethane, and 0.1-0.5 parts of amine catalyst.

[0009] Preferably, the polyether polyol is PPG2000, and its hydroxyl value is 54-58 mgKOH / g;

[0010] The hydrophilic agent is ZL-480; the pore opening agent is ZL Y-1900; and the amine catalyst is N-methyldiethanolamine.

[0011] Preferably, the konjac glucomannan-acrylic acid graft copolymer is prepared by the following method:

[0012] Potassium persulfate was used as an initiator and N,N'-methylenebisacrylamide was used as a crosslinking agent. 10.0 g of konjac glucomannan and 100 mL of acrylic acid neutralized with sodium hydroxide were added into a 500 mL three-necked bottle, stirred at 35 degrees for 1 hour under nitrogen protection until the konjac flour expanded, then 0.5 g of initiator and 0.08 g of crosslinking agent were added, stirred evenly, and then placed in a water bath at 60°C for uniform reaction for 2 hours, and the product was taken out, dried, crushed, and sieved to obtain konjac glucomannan-acrylic acid graft copolymer.

[0013] Konjac is a special resource in China. Its main component is konjac glucomannan (KGM), a heteropolysaccharide composed of glucose and mannose connected by β-glycosidic bonds, which has good water absorption and moisture retention. In this study, we modified konjac glucomannan and grafted it with acrylic acid to synthesize konjac glucomannan-propionic acid graft copolymer (KSAP), which contains a large number of hydrophilic groups such as hydroxyl and carboxyl groups.

[0014] Another object of the present invention is to provide a method for preparing the above-mentioned hydrophilic polyurethane filler, comprising:

[0015] The polyether polyol, amine catalyst, dibutyltin dilaurate, silicone foam stabilizer, water, dichloromethane, hydrophilic agent, pore opening agent, konjac glucomannan-acrylic acid graft copolymer are weighed in sequence in a container, stirred evenly, and allowed to stand. The weighed diphenylmethane diisocyanate is then added to the container, stirred for 5-15 seconds, and poured into a foaming box for free foaming. After the foaming stops, the container is placed in an oven for further foaming for 60 minutes, and then allowed to stand for 24 hours to obtain the hydrophilic polyurethane filler.

[0016] Preferably, the temperature of the oven is 55-65°C.

[0017] Preferably, the stirring time is 3 minutes and the stirring speed is 150 rpm / min.

[0018] Preferably, the standing time is 1 min.

[0019] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. Provides a method for preparing polyurethane filler with simple operation and low cost;

[0021] 2. The hydrophilic polyurethane sponge of the present invention has good hydrophilic effect and good film-forming effect;

[0022] 3. The hydrophilic polyurethane sponge of the present invention is added with a unique natural polymer material konjac and acrylic acid grafted modified product konjac glucomannan-acrylic acid graft copolymer (KSAP), which has a good effect of improving the hydrophilicity of the polyurethane sponge. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0024] Figure 1 This is a comparison chart of the film formation amount of different fillers. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] This embodiment provides a hydrophilic polyurethane filler, including the following components in parts by weight:

[0028] 100 parts of polyether polyol (PPG2000, hydroxyl value 58 mgKOH / g), 60 parts of MDI (diphenylmethane diisocyanate), 30 parts of hydrophilic agent (ZL-480), 15 parts of pore opener (ZL Y-1900), 3 parts of konjac glucomannan-acrylic acid graft copolymer, 1 part of dibutyltin dilaurate, 1 part of silicone foam stabilizer, 1.25 parts of water, 0.75 parts of dichloromethane, and 0.3 parts of N-methyldiethanolamine.

[0029] Example 2

[0030] This embodiment provides a hydrophilic polyurethane filler, including the following components in parts by weight:

[0031] 105 parts of polyether polyol (PPG2000, hydroxyl value 54 mgKOH / g), 55 parts of MDI (diphenylmethane diisocyanate), 35 parts of hydrophilic agent (ZL-480), 10 parts of pore opener (ZL Y-1900), 2 parts of konjac glucomannan-acrylic acid graft copolymer, 2 parts of dibutyltin dilaurate, 1 part of silicone foam stabilizer, 1 part of water, 1 part of dichloromethane, and 0.1 part of N-methyldiethanolamine.

[0032] Example 3

[0033] This embodiment provides a hydrophilic polyurethane filler, including the following components in parts by weight:

[0034] 95 parts of polyether polyol (PPG2000, hydroxyl value 55 mgKOH / g), 65 parts of MDI (diphenylmethane diisocyanate), 25 parts of hydrophilic agent (ZL-480), 20 parts of pore opener (ZL Y-1900), 4 parts of konjac glucomannan-acrylic acid graft copolymer, 1 part of dibutyltin dilaurate, 1 part of silicone foam stabilizer, 0.5 parts of water, 0.5 parts of dichloromethane, and 0.5 parts of N-methyldiethanolamine.

[0035] Example 4

[0036] This embodiment provides a method for preparing a hydrophilic polyurethane filler, comprising the following steps:

[0037] Preparation of konjac glucomannan-propionic acid graft copolymer (KSAP): Potassium persulfate is used as an initiator and N,N'-methylenebisacrylamide is used as a crosslinking agent. 10.0g of konjac glucomannan and 100mL of acrylic acid neutralized with sodium hydroxide are added into a 500ml three-necked bottle, stirred at 35 degrees for 1h under nitrogen protection until the konjac flour expands, then 0.5g of initiator and 0.08g of crosslinking agent are added, stirred evenly, and then placed in a water bath at 60°C for uniform reaction for 2h, and the product is taken out, dried, crushed and sieved to obtain konjac glucomannan-acrylic acid graft copolymer.

[0038] According to any one of the formulations in Examples 1-3, polyether polyol, N-methyldiethanolamine, dibutyltin dilaurate, silicone foam stabilizer, water, dichloromethane, hydrophilic agent, pore opening agent, and konjac glucomannan-acrylic acid graft copolymer were weighed in a beaker in sequence, stirred evenly with an electric stirrer, and allowed to stand for a while. The whole process was controlled at room temperature of 25°C. The weighed MDI was quickly added to the beaker, stirred for 10 seconds, and then poured into a foaming box for free foaming. After the foaming stopped, it was placed in a 60-degree oven for foaming for 60 minutes. After the foaming stopped, it was placed at room temperature for 24 hours and cut into multiple 200mm×200mm×200mm cubes.

[0039] Performance Testing

[0040] The properties of the hydrophilic polyurethane filler prepared by the formula of Example 1 were measured, and the water absorption rate, sedimentation time, tensile strength, open porosity, etc. of the polyurethane filler were determined by the following methods.

[0041] Water absorption test: first use an electronic balance to weigh the mass m1 of a prepared filler, then throw a piece of filler into the water, take it out after half an hour, use filter paper to absorb the surface water, and weigh the mass m2. Water absorption = (m2-m1) / m1×100%.

[0042] The tensile strength is tested according to the method of GB / T 6344-2008 (test of tensile strength and elongation at break of soft foam polymer materials); the open porosity is tested according to the method of GB / T 10799-2008 (determination of the volume percentage of open and closed cells of rigid foam plastics).

[0043] The measured results are shown in Table 1:

[0044] Table 1

[0045]

[0046]

[0047] Effect of the dosage of konjac glucomannan-acrylic acid graft copolymer on the hydrophilicity of fillers

[0048] According to the formulation shown in Example 1, the other ingredients except the konjac glucomannan-acrylic acid graft copolymer were kept unchanged, the composition of the konjac glucomannan-acrylic acid graft copolymer was changed, and the effect of the amount of the konjac glucomannan-acrylic acid graft copolymer on the hydrophilicity and physical properties of the sponge was investigated. The results are shown in Table 2.

[0049] Table 2

[0050]

[0051] As shown in Table 2, when not adding konjak glucomannan-acrylic acid graft copolymer, the water absorption of prepared hydrophilic filler is relatively low, and the settling time in water is relatively long. Along with the increase of konjak glucomannan-acrylic acid graft copolymer consumption, the water absorption of prepared hydrophilic polyurethane filler significantly improves, and its settling time in water is also obviously shortened. This may be due to the foaming reaction that konjak glucomannan-acrylic acid graft copolymer participates in the polyurethane preparation process, and the hydrophilic segment is introduced into the polyurethane molecular segment, improves the hydrophilic ability of sponge, and its water absorption increases, so that the sponge increases due to water absorption and self quality, thereby shortens the settling time in water.

[0052] Effect of the dosage of hydrophilic agent ZL-480 on the hydrophilic properties of fillers

[0053] According to the formulation shown in Example 1, by keeping other ingredients unchanged and changing the ingredients of the hydrophilic agent ZL-480, the effect of the amount of the hydrophilic agent ZL-480 on the hydrophilicity and physical properties of the filler was investigated. The results are shown in Table 3.

[0054] Table 3

[0055]

[0056] It can be seen from Table 3 that if ZL-480 is not added, that is, when the content of ZL-480 is 0, the water absorption rate of the prepared filler is relatively low, only 31%, and the sedimentation time in water is relatively long. As the content of ZL-480 increases, the water absorption rate of the prepared hydrophilic sponge is significantly improved, and its sedimentation time in water is significantly shortened. This is also because ZL-480 participates in the foaming reaction, introduces the hydrophilic segment into the polyurethane molecular segment, and improves the hydrophilic ability of the sponge. When the dosage of ZL-480 is 45 parts, the water absorption rate and sedimentation time of the filler are not much different from when the dosage of ZL-480 is 30. Therefore, the dosage of ZL-480 is selected to be 30 parts.

[0057] Effect of the dosage of amine catalyst N-methyldiethanolamine on filler properties

[0058] Table 4

[0059]

[0060] It can be seen from Table 4 that when the amount of N-methyldiethanolamine is 0.1-0.3 parts, as the amount of N-methyldiethanolamine increases, the tensile strength of the prepared filler increases accordingly. This is because tertiary amine catalysts have a strong catalytic effect, which can promote the reaction of -NCO and -OH, promote the rapid growth of polymer molecular chains, rapidly increase viscosity, and rapidly improve the strength of the foam network skeleton. As the amount of N-methyldiethanolamine increases, polyurethane foam collapse reaction occurs, because the increase in the amount of N-methyldiethanolamine causes -NCO to react with water too quickly, thereby causing the speed of generating carbon dioxide gas to be too fast, and ultimately leading to foam collapse reaction.

[0061] Comparative experiment on the biofilm formation of different fillers on the market

[0062] Prepare three 1L beakers, marked as samples 1, 2, and 3. Add 500ML of activated sludge to each beaker, and add 2 different fillers to each beaker. Sample 1 is Qingdao Banghao filler, sample 2 is Kong Lingcai hydrophobic filler, and sample 3 is Example 1 filler. These three groups of samples need to be weighed by weight and volume before the experiment. After adding to the beaker, the filler will adsorb the sludge through physical adsorption. After waiting for 4 hours, take out all the fillers, bake them in an oven at 100 degrees for 10 hours, and then weigh them. In this way, the amount of biofilm in each group of fillers is obtained. The results are as follows. Figure 1 shown.

[0063] Depend on Figure 1 As far as we know, the filler produced in this experiment has the best biofilm amount, followed by Qingdao Banghao filler, and the worst biofilm amount is Kong Lingcai hydrophobic filler.

[0064] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0065] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A hydrophilic polyurethane filler, characterized in that: It includes the following components by weight: 95-105 parts of polyether polyol, 55-65 parts of diphenylmethane diisocyanate, 25-35 parts of hydrophilic agent, 10-20 parts of cell opener, 2-4 parts of konjac glucomannan-acrylic acid graft copolymer, 1-2 parts of dibutyltin dilaurate, 1-2 parts of organosilicon foam stabilizer, 1-2 parts of water, 0.5-1 parts of dichloromethane, and 0.1-0.5 parts of amine catalyst; The polyether polyol is PPG2000, and its hydroxyl value is 54-58 mgKOH / g; The hydrophilic agent is ZL-480; the pore opening agent is ZL Y-1900; the amine catalyst is N-methyldiethanolamine; The konjac glucomannan-acrylic acid graft copolymer is prepared by the following method: Using potassium persulfate as initiator and N,N'-methylenebisacrylamide as cross-linking agent, 10.0g of konjac glucomannan and 100mL of acrylic acid neutralized with sodium hydroxide were added into a 500-ml three-necked flask, and stirred at 35 degrees for 1 hour under nitrogen protection until the konjac flour expanded. Subsequently, 0.5g of initiator and 0.08g of cross-linking agent were added, and after stirring evenly, the mixture was placed in a water bath at 60°C and reacted evenly for 2 hours. The product was taken out, dried, crushed and sieved to obtain konjac glucomannan-acrylic acid graft copolymer.

2. The method for preparing a hydrophilic polyurethane filler according to claim 1, characterized in that: include: The polyether polyol, amine catalyst, dibutyltin dilaurate, silicone foam stabilizer, water, dichloromethane, hydrophilic agent, pore opening agent, konjac glucomannan-acrylic acid graft copolymer are weighed in sequence in a container, stirred evenly, and allowed to stand. The weighed diphenylmethane diisocyanate is then added to the container, stirred for 5-15 seconds, and poured into a foaming box for free foaming. After the foaming stops, the container is placed in an oven for further foaming for 60 minutes, and then allowed to stand for 24 hours to obtain the hydrophilic polyurethane filler.

3. The method for preparing a hydrophilic polyurethane filler according to claim 2, characterized in that: The temperature of the oven is 55-65°C.

4. The method for preparing a hydrophilic polyurethane filler according to claim 2, characterized in that: The stirring time is 3 minutes and the stirring speed is 150 rpm / min.

5. The method for preparing a hydrophilic polyurethane filler according to claim 2, characterized in that: The standing time is 1 min.

Citation Information

Patent Citations

  • Environment degrading thermalplastic glucomanan foam material and moulding process thereof

    CN101497732A

  • Medical hydrogel foam dressing and preparation method thereof

    CN106729956A

  • Flame-retardant polyurethane material, processing method thereof, and flame retardant thereof

    CN107033581A

  • Process for making flexible foams

    CN1164243A

  • Konjaku plucosidopolyose graft copolymer, preparing process and use thereof

    CN1401678A