A heating element integrated porous ceramic heating body

Through the design of the double-layer structure and high-temperature resistant and anti-oxidation coating, the problem of oxidation corrosion of the porous ceramic heating element at high temperatures is solved, the service life is extended and the structural stability is improved.

CN117596728BActive Publication Date: 2024-10-01SHENGYE TEBANG (SHENZHEN) IND DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311563650.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-21
Publication Date
2024-10-01
Estimated Expiration
2043-11-21

AI Technical Summary

Technical Problem

When the existing porous ceramic heating element is heated at high temperature, the conductive circuit reacts with oxygen in the air, causing oxidative corrosion and reducing the service life.

Method used

An integrated porous ceramic heating element with a double-layer structure is used. A conductive metal layer is set between the outer and inner ceramic layers, and holes are hollowed out on the surface. Both sides are coated with high-temperature-resistant and anti-oxidation coatings, which are pressed and sintered. Process preparation.

Benefits of technology

It effectively protects the conductive metal layer, improves oxidation resistance, extends service life, and uses the low thermal expansion coefficient of ceramics to stabilize the volume change of the conductive metal layer and enhance structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117596728B_ABST
    Figure CN117596728B_ABST
Patent Text Reader

Abstract

The present invention discloses a heating element integrated porous ceramic heating body, which relates to the technical field of dental comprehensive treatment machines; in order to solve the life problem; it specifically includes an outer porous ceramic located at the outermost side, an inner porous ceramic located at the innermost side, and a conductive metal layer arranged on the opposite side of the outer porous ceramic and the inner porous ceramic. The present invention arranges a double-layer arrangement of an inner porous ceramic located at the inner side and an outer porous ceramic located at the outer side, which can better protect the conductive metal layer on the one hand, and with the high temperature resistant and anti-oxidation coating, it can have good oxidation resistance and increase the service life, and the arrangement of the inner and outer layers can utilize the characteristics of the low thermal expansion coefficient of the ceramic itself to limit and suppress the volume change of the conductive metal layer when it is heated or cooled, thereby increasing the stability of the structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic atomization, and in particular to a heating element integrated porous ceramic heating body. Background Art

[0002] Porous ceramics are ceramic materials with many small pores, and their porosity can reach 60-90%. Porous ceramics have excellent chemical stability, high temperature oxidation resistance, thermal resistance, high strength and low thermal expansion coefficient, so they are widely used in catalyst carriers, foamed ceramics, filter materials, biomedical materials, electronic devices and other fields.

[0003] An electronic atomizer is a device that uses a ceramic heating element to heat the atomized liquid to produce a smokeable aerosol. It is mainly used as a smoking substitute or a medical suction device.

[0004] For example, after searching, the Chinese patent publication number CN115124323B discloses a porous ceramic heating element and a preparation method thereof, including raw materials: ceramic powder, low-temperature glass powder, pore-forming agent, adhesive and surfactant; the heating component includes a carbon fiber unidirectional tape and a conductive circuit printed on the carbon fiber unidirectional tape.

[0005] The above patent has the following shortcomings: it adopts a single-layer arrangement, which will cause the conductive circuit and the heating component to be partially placed in the air. When heated at high temperature, it will react with the oxygen in the air, causing oxidative corrosion and reducing the service life.

[0006] To this end, the present invention proposes a heating element integrated porous ceramic heating body. Summary of the invention

[0007] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a heating element integrated porous ceramic heating body.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A heating element integrated porous ceramic heating body, comprising an outer porous ceramic layer located at the outermost side, an inner porous ceramic layer located at the innermost side, and a conductive metal layer arranged between the outer porous ceramic layer and the inner porous ceramic layer;

[0010] The surface of the conductive metal layer is provided with uniform hollow holes, and an electrode ear is welded to one end surface of the conductive metal layer, and an electrode is welded to the other end of the electrode;

[0011] The outer side of the outer porous ceramic, the inner side of the inner porous ceramic, the inner side of the hollow hole and the two end surfaces of the conductive metal layer are all provided with high temperature resistant and anti-oxidation coatings.

[0012] Preferably: the method for preparing the porous ceramic heating element comprises the following steps:

[0013] S1: preparing raw materials for outer porous ceramic and inner porous ceramic, preparing raw materials for preparing outer porous ceramic and inner porous ceramic;

[0014] S2: Preliminary forming, placing the conductive metal layer in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer, and then using the pressing device to perform pressing forming;

[0015] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0016] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0017] Furthermore: in the step S1, the raw materials include basic materials and additives.

[0018] Based on the above solution: the base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0019] A more preferred embodiment of the aforementioned embodiment is that the additives include a binder, a template and an active agent.

[0020] As a further solution of the present invention: the adhesive is polyvinyl alcohol or polyacrylate, the template is latex particles or hard particles, and the active agent is ammonium nitrate or sodium nitrate.

[0021] Meanwhile, in the step S1, the proportions of the various raw materials are: 60% to 90% alumina, 0% to 1.5% zirconium oxide, 1% to 5% adhesive, 5% to 20% template, and 1% to 10% active agent.

[0022] As a preferred embodiment of the present invention: the high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

[0023] Meanwhile, the composition ratios of the adhesive, high temperature resistant and antioxidant material and additive are 20% to 40%, 40% to 70% and 1% to 10%.

[0024] As a more optimal solution of the present invention: the adhesive is silicate, the high temperature resistant and antioxidant material is aluminum oxide, and the additives include dispersants, thickeners, leveling agents, drying aids, anti-settling agents and anti-pollution agents.

[0025] The beneficial effects of the present invention are:

[0026] The present invention, by arranging a double-layer arrangement of an inner porous ceramic layer located on the inside and an outer porous ceramic layer located on the outside, can better protect the conductive metal layer on the one hand, and with the high-temperature resistant and anti-oxidation coating, can have better oxidation resistance and increase the service life. In addition, the inner and outer two-layer arrangement can utilize the low thermal expansion coefficient of the ceramic itself to limit and suppress the volume change of the conductive metal layer when it is heated or cooled, thereby increasing the stability of the structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the exploded structure of a heating element integrated porous ceramic heating body proposed by the present invention.

[0028] In the figure: outer porous ceramic 1, conductive metal layer 2, hollow hole 3, electrode ear 4, electrode 5, inner porous ceramic 6. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.

[0030] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0031] Embodiment 1:

[0032] A heating element integrated porous ceramic heating body, such as Figure 1 As shown, it includes an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6 .

[0033] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0034] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0035] In this embodiment, a double-layer arrangement of an inner porous ceramic 6 located on the inner side and an outer porous ceramic 1 located on the outer side can better protect the conductive metal layer 2 on the one hand, and with the high-temperature resistant and anti-oxidation coating, it can have better oxidation resistance and increase the service life. In addition, by adopting an inner and outer two-layer arrangement, the low thermal expansion coefficient of the ceramic itself can be used to limit and suppress the volume change of the conductive metal layer 2 when heated or cooled, thereby increasing the stability of the structure.

[0036] Embodiment 2:

[0037] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0038] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0039] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0040] The preparation method comprises the following steps:

[0041] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0042] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0043] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0044] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0045] In the step S1, the raw materials include basic materials and additives.

[0046] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0047] The additives include a binder, a template and an active agent.

[0048] The adhesive is polyvinyl alcohol or polyacrylate.

[0049] The template is latex particles or hard particles.

[0050] The active agent is ammonium nitrate or sodium nitrate.

[0051] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0052] Embodiment 3:

[0053] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0054] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0055] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0056] The preparation method comprises the following steps:

[0057] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0058] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0059] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0060] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0061] In the step S1, the raw materials include basic materials and additives.

[0062] The base material is alumina.

[0063] The additives include a binder, a template and an active agent.

[0064] The adhesive is polyvinyl alcohol.

[0065] The template is latex particles.

[0066] The active agent is ammonium nitrate.

[0067] Embodiment 4:

[0068] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0069] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0070] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0071] The preparation method comprises the following steps:

[0072] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0073] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0074] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0075] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0076] In the step S1, the raw materials include basic materials and additives.

[0077] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0078] The additives include a binder, a template and an active agent.

[0079] The adhesive is polyacrylate.

[0080] The template is hard particles.

[0081] The active agent is sodium nitrate.

[0082] Embodiment 5:

[0083] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0084] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0085] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0086] The preparation method comprises the following steps:

[0087] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0088] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0089] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0090] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0091] In the step S1, the raw materials include basic materials and additives.

[0092] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0093] The additives include a binder, a template and an active agent.

[0094] The adhesive is polyvinyl alcohol or polyacrylate.

[0095] The template is latex particles or hard particles.

[0096] The active agent is ammonium nitrate or sodium nitrate.

[0097] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0098] Embodiment 6:

[0099] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0100] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0101] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0102] The preparation method comprises the following steps:

[0103] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0104] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0105] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0106] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0107] In the step S1, the raw materials include basic materials and additives.

[0108] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0109] The additives include a binder, a template and an active agent.

[0110] The adhesive is polyvinyl alcohol or polyacrylate.

[0111] The template is latex particles or hard particles.

[0112] The active agent is ammonium nitrate or sodium nitrate.

[0113] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0114] Embodiment 7:

[0115] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0116] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0117] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0118] The preparation method comprises the following steps:

[0119] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0120] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0121] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0122] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0123] In the step S1, the raw materials include basic materials and additives.

[0124] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0125] The additives include a binder, a template and an active agent.

[0126] The adhesive is polyvinyl alcohol or polyacrylate.

[0127] The template is latex particles or hard particles.

[0128] The active agent is ammonium nitrate or sodium nitrate.

[0129] In the step S1, the proportions of the various raw materials are: 70% to 80% of aluminum oxide, 0% to 1.5% of zirconium oxide, 2% to 4% of adhesive, 10% to 15% of template, and 3% to 8% of active agent.

[0130] Embodiment 8:

[0131] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0132] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0133] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0134] The preparation method comprises the following steps:

[0135] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0136] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0137] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0138] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0139] In the step S1, the raw materials include basic materials and additives.

[0140] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0141] The additives include a binder, a template and an active agent.

[0142] The adhesive is polyvinyl alcohol or polyacrylate.

[0143] The template is latex particles or hard particles.

[0144] The active agent is ammonium nitrate or sodium nitrate.

[0145] In the step S1, the proportions of the various raw materials are: 75% alumina, 0% to 1.5% zirconium oxide, 3% adhesive, 12.5% ​​template, and 5% active agent.

[0146] Embodiment 9:

[0147] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0148] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0149] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0150] The preparation method comprises the following steps:

[0151] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0152] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0153] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0154] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0155] In the step S1, the raw materials include basic materials and additives.

[0156] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0157] The additives include a binder, a template and an active agent.

[0158] The adhesive is polyvinyl alcohol or polyacrylate.

[0159] The template is latex particles or hard particles.

[0160] The active agent is ammonium nitrate or sodium nitrate.

[0161] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0162] The high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

[0163] The composition ratios of the adhesive, the high temperature resistant and antioxidant material and the additive are 20% to 40%, 40% to 70% and 1% to 10%.

[0164] Example 10

[0165] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0166] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0167] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0168] The preparation method comprises the following steps:

[0169] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0170] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0171] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0172] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0173] In the step S1, the raw materials include basic materials and additives.

[0174] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0175] The additives include a binder, a template and an active agent.

[0176] The adhesive is polyvinyl alcohol or polyacrylate.

[0177] The template is latex particles or hard particles.

[0178] The active agent is ammonium nitrate or sodium nitrate.

[0179] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0180] The high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

[0181] The composition ratios of the adhesive, high temperature resistant and antioxidant material and additive are 25% to 35%, 50% to 60% and 3% to 7%.

[0182] Embodiment 11

[0183] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0184] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0185] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0186] The preparation method comprises the following steps:

[0187] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0188] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0189] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0190] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0191] In the step S1, the raw materials include basic materials and additives.

[0192] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0193] The additives include a binder, a template and an active agent.

[0194] The adhesive is polyvinyl alcohol or polyacrylate.

[0195] The template is latex particles or hard particles.

[0196] The active agent is ammonium nitrate or sodium nitrate.

[0197] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0198] The high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

[0199] The composition ratios of the adhesive, high temperature resistant and antioxidant material and additive are 30%, 55% and 5% respectively.

[0200] Embodiment 12:

[0201] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0202] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0203] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0204] The preparation method comprises the following steps:

[0205] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0206] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0207] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0208] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0209] In the step S1, the raw materials include basic materials and additives.

[0210] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0211] The additives include a binder, a template and an active agent.

[0212] The adhesive is polyvinyl alcohol or polyacrylate.

[0213] The template is latex particles or hard particles.

[0214] The active agent is ammonium nitrate or sodium nitrate.

[0215] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0216] The high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

[0217] The composition ratios of the adhesive, the high temperature resistant and antioxidant material and the additive are 20% to 40%, 40% to 70% and 1% to 10%.

[0218] The adhesive is aluminate.

[0219] The high temperature resistant and oxidation resistant material is zirconium oxide.

[0220] The additives include dispersants, thickeners, leveling agents, drying aids, anti-settling agents and anti-pollution agents.

[0221] Embodiment 13:

[0222] A heating element integrated porous ceramic heating body comprises an outer porous ceramic 1 located at the outermost side, an inner porous ceramic 6 located at the innermost side, and a conductive metal layer 2 arranged between the outer porous ceramic 1 and the inner porous ceramic 6.

[0223] The surface of the conductive metal layer 2 is provided with uniform hollow holes 3 , and an electrode ear 4 is welded to one end surface of the conductive metal layer 2 , and an electrode 5 is welded to the other end surface of the conductive metal layer 2 .

[0224] The outer side of the outer porous ceramic 1 , the inner side of the inner porous ceramic 6 , the inner side of the hollow hole 3 , and the two end surfaces of the conductive metal layer 2 are all provided with high temperature resistant and anti-oxidation coatings.

[0225] The preparation method comprises the following steps:

[0226] S1: preparing raw materials for the outer porous ceramic 1 and the inner porous ceramic 6, preparing raw materials for preparing the outer porous ceramic 1 and the inner porous ceramic 6;

[0227] S2: Preliminary forming, placing the conductive metal layer 2 in the concave mold of the pressing device, then spreading the raw materials on the inner and outer sides of the conductive metal layer 2, and then using the pressing device to perform pressing forming;

[0228] S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere;

[0229] S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

[0230] In the step S1, the raw materials include basic materials and additives.

[0231] The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

[0232] The additives include a binder, a template and an active agent.

[0233] The adhesive is polyvinyl alcohol or polyacrylate.

[0234] The template is latex particles or hard particles.

[0235] The active agent is ammonium nitrate or sodium nitrate.

[0236] In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

[0237] The high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

[0238] The composition ratios of the adhesive, the high temperature resistant and antioxidant material and the additive are 20% to 40%, 40% to 70% and 1% to 10%.

[0239] The adhesive is silicate.

[0240] The high temperature resistant and oxidation resistant material is aluminum oxide.

[0241] The additives include dispersants, thickeners, leveling agents, drying aids, anti-settling agents and anti-pollution agents.

[0242] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A heating element integrated porous ceramic heating body, characterized in that: It comprises an outer porous ceramic (1) located at the outermost side, an inner porous ceramic (6) located at the innermost side, and a conductive metal layer (2) arranged between the outer porous ceramic (1) and the inner porous ceramic (6); The surface of the conductive metal layer (2) is provided with uniform hollow holes (3), and an electrode ear (4) is welded to one end surface of the conductive metal layer (2), and an electrode (5) is welded to the other end of the electrode (5); The outer side of the outer porous ceramic (1), the inner side of the inner porous ceramic (6), the inner side of the hollow hole (3) and the two end surfaces of the conductive metal layer (2) are all provided with high temperature resistant and anti-oxidation coatings; The preparation method of the porous ceramic heating element comprises the following steps: S1: preparing raw materials for the outer layer porous ceramic (1) and the inner layer porous ceramic (6), preparing raw materials for preparing the outer layer porous ceramic (1) and the inner layer porous ceramic (6); S2: Preliminary forming, placing the conductive metal layer (2) in a concave mold of a pressing device, spreading raw materials on the inner and outer sides of the conductive metal layer (2), and then performing pressing forming using a pressing device; S3: Secondary consolidation: placing the initially pressed blank into a sintering furnace and sintering it in a protective gas atmosphere; S4: Infiltration coating: Place the sintered blank into the high temperature resistant and anti-oxidation coating for infiltration, then take it out and dry it.

2. The heating element integrated porous ceramic heating body according to claim 1, characterized in that: In the step S1, the raw materials include basic materials and additives.

3. The heating element integrated porous ceramic heating body according to claim 2, characterized in that: The base material is aluminum oxide or a mixture of aluminum oxide and zirconium oxide.

4. The heating element integrated porous ceramic heating body according to claim 2, characterized in that: The additives include a binder, a template and an active agent.

5. The heating element integrated porous ceramic heating body according to claim 4, characterized in that: The adhesive is polyvinyl alcohol or polyacrylate, the template is latex particles or hard particles, and the active agent is ammonium nitrate or sodium nitrate.

6. The heating element integrated porous ceramic heating body according to claim 5, characterized in that: In the step S1, the proportions of the various raw materials are: 60% to 90% of aluminum oxide, 0% to 1.5% of zirconium oxide, 1% to 5% of adhesive, 5% to 20% of template, and 1% to 10% of active agent.

7. The heating element integrated porous ceramic heating body according to claim 1, characterized in that: The high temperature resistant and anti-oxidation coating comprises an adhesive, a high temperature resistant and anti-oxidation material and an additive.

8. The heating element integrated porous ceramic heating body according to claim 7, characterized in that: The composition ratios of the adhesive, the high temperature resistant and antioxidant material and the additive are 20% to 40%, 40% to 70% and 1% to 10%.

9. The heating element integrated porous ceramic heating body according to claim 8, characterized in that: The adhesive is silicate, the high temperature resistant and anti-oxidation material is aluminum oxide, and the additives include a dispersant, a thickener, a leveling agent, a drying aid, an anti-settling agent and an anti-pollution agent.