A method for preparing an antistatic double-layer composite wire tube
By using a double-layer composite structure and specific formula materials in plastic wire pipes, the heat resistance, low temperature performance and color problems of existing wire pipes are solved, and the anti-static, aging resistance and strength are improved, ensuring that wire pipes are in the market Competitive on.
Patent Information
- Application Number
- CN202311836297.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-12-27
AI Technical Summary
The existing plastic wire tube materials have shortcomings in terms of heat resistance and low temperature performance, and conductive additives cause the wire tube to turn black, affecting market sales.
Using a double-layer composite structure, the inner layer is prepared by PVC, conductive carbon black, ABS resin and SAN-b-PVC compatibility agent, and the outer layer is PVC, 2,6-di-tert-butyl-4-allyl phenol, Preparation of diisopropyl oxide and ASA resin, anti-static double-layer composite wire tubes are prepared by melt premix and double-layer coextrusion to ensure that the wire tubes maintain a white appearance while ensuring anti-static properties.
It has achieved comprehensive performance improvements in anti-static, aging resistance, heat resistance, low temperature resistance and strength, ensuring that the wire pipes are competitive in the market.
Smart Images

Figure CN117601387B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic wire tubes, and in particular to a method for preparing an antistatic double-layer composite wire tube. Background Art
[0002] At present, the main material of wire tubes is polyvinyl chloride (PVC). PVC pipes have good tensile and compressive strength, but poor heat resistance and are brittle at low temperatures. In addition, static electricity is a safety hazard in circuit systems, so the wire tube materials used must have good antistatic properties, which are usually achieved by adding conductive graphite, conductive carbon black, and coating with electrostatic shielding coatings. However, the blending of conductive graphite, conductive carbon black and the wire tube substrate makes the wire tube black, and the shielding coating is not easy to coat on the inner surface of the wire tube. It is mostly coated on the outer surface of the wire tube, but black wire tubes are difficult to sell. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a method for preparing an antistatic double-layer composite wire pipe. The obtained composite wire pipe has the properties of antistatic, aging resistance, heat resistance, low temperature resistance, high strength, etc., has a white appearance, and is competitive in the market.
[0004] In order to achieve the above object, the present invention adopts the following technical solution:
[0005] A method for preparing an antistatic double-layer composite wire tube comprises the following steps:
[0006] (a) PVC resin, conductive carbon black, ABS resin, and SAN-b-PVC compatibilizer are prepared in proportion as the raw materials for the inner layer; PVC resin, 2,6-di-tert-butyl-4-allylphenol, diisopropylbenzene peroxide, and ASA resin are prepared in proportion and mixed evenly as the raw materials for the outer layer;
[0007] (b) melt premixing the inner layer raw material and the outer layer raw material respectively by using a melt premixing device;
[0008] (c) The two pre-melts of step (b) are respectively input into a screw extruder and extruded by a double-layer co-extrusion method, and after cooling and molding, an antistatic double-layer composite wire tube is obtained.
[0009] In step (a), based on 100% of the total mass of the inner layer raw materials, the inner layer raw materials include 62.4-68.5% of PVC resin, 7.5-10% of conductive carbon black, 17-21.5% of ABS resin, and 6.5-8.6% of SAN-b-PVC compatibilizer.
[0010] In step (a), based on 100% of the total mass of the outer layer raw materials, the outer layer raw materials include 79.6-81.15% of PVC resin, 0.2-0.3% of 2,6-di-tert-butyl-4-allyl phenol, 0.1-0.2% of diisopropylbenzene peroxide, and 16.4-20% of ASA resin.
[0011] In step (b), the temperature of the melt premixing of the inner layer raw material and the outer layer raw material is 165-170°C.
[0012] During the extrusion of the inner layer raw material in step (c), the temperatures of zones 1 to 5 of the extruder are 160-165° C., 165-170° C., 170-175° C., 175-180° C., and 180-185° C., respectively.
[0013] During the extrusion of the outer layer raw material in step (c), the temperatures of zones 1 to 5 of the extruder are 160-164° C., 164-170° C., 170-175° C., 175-180° C., and 180-185° C., respectively.
[0014] During double-layer co-extrusion, the co-extrusion die temperature is controlled at 185°C.
[0015] The cooling molding temperature is 20-30℃.
[0016] The beneficial effects of the present invention are as follows: the inner layer is blended with ABS and PVC, and SAN-b-PVC is used as a compatibilizer to improve the aging resistance, heat resistance and low-temperature brittleness of the inner layer PVC; the outer layer is blended with PVC and ASA to improve the aging resistance, heat resistance and low-temperature brittleness of the outer layer PVC; conductive carbon black is added to the inner layer, and the appearance can be kept white while ensuring the antistatic performance, thereby ensuring the market competitiveness; and the inner layer ABS material can be copolymerized with the outer layer 2,6-di-tert-butyl-4-allylphenol material under the action of an initiator to generate a modified acrylonitrile-butadiene-styrene copolymer, thereby effectively promoting the bonding strength between the inner layer and the outer layer, thereby ensuring the strength performance of the wire tube. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a structural diagram of the melt premix of the present invention;
[0018] Figure 2 for Figure 1 The enlarged view of point A in the middle;
[0019] Figure 3 for Figure 1 The enlarged view of point B in the middle;
[0020] Figure 4 for Figure 1 Partial cross-section along CC direction.
[0021] In the figure: bracket 1, outer cylinder 2, sleeve 21, gear ring 22, slide rail 23, push plate 3, dispersion plate 4, scattering hole 41, mounting frame 5, drive shaft 6, A gear 61, bevel gear assembly 62, rotating shaft 7, slider 8, motor 9. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments:
[0023] The antistatic double-layer composite wire tube of the present invention is prepared according to the following steps:
[0024] (a) PVC resin, conductive carbon black, ABS resin, and SAN-b-PVC compatibilizer are prepared in proportion as the raw materials for the inner layer; PVC resin, 2,6-di-tert-butyl-4-allylphenol, diisopropylbenzene peroxide, and ASA resin are prepared in proportion and mixed evenly as the raw materials for the outer layer; based on 100% of the total mass of the raw materials for the inner layer, the raw materials for the inner layer include 62.4-68.5% of PVC resin, 7.5-10% of conductive carbon black, 17-21.5% of ABS resin, and 6.5-8.6% of SAN-b-PVC compatibilizer. Based on 100% of the total mass of the raw materials for the outer layer, the raw materials for the outer layer include 79.6-81.15% of PVC resin, 0.2-0.3% of 2,6-di-tert-butyl-4-allylphenol, 0.1-0.2% of diisopropylbenzene peroxide, and 16.4-20% of ASA resin.
[0025] (b) melt premixing devices are used to melt premix the inner layer raw materials and the outer layer raw materials respectively; the melt premixing temperatures of the inner layer raw materials and the outer layer raw materials are both 165-170°C.
[0026] (c) The two pre-melts of step (b) are respectively input into a screw extruder, and extruded by a double-layer co-extrusion method, and an antistatic double-layer composite wire tube is obtained after cooling and molding. When the inner layer raw material is extruded, the temperatures of the first to fifth zones of the extruder are 160-165°C, 165-170°C, 170-175°C, 175-180°C, and 180-185°C, respectively. When the outer layer raw material is extruded, the temperatures of the first to fifth zones of the extruder are 160-164°C, 164-170°C, 170-175°C, 175-180°C, and 180-185°C, respectively. During double-layer co-extrusion, the co-extrusion die temperature is controlled to be 185°C. The cooling molding temperature is 20-30°C.
[0027] According to the above preparation method and the proportions and adjustments described in Table 1, an antistatic double-layer composite wire tube is produced.
[0028] Table 1
[0029]
[0030] The performance of the antistatic double-layer composite wire tubes prepared in Examples 1-5 was tested, and the results are shown in Table 2.
[0031] Table 2
[0032]
[0033]
[0034] In the present invention, the raw materials need to be uniformly mixed and melted. However, in the prior art, melt mixing is mostly performed by screw extruders, and the mixing effect is not very ideal, resulting in uneven material distribution and affecting product performance. In the embodiment of the present invention, a method of pre-melting and then screw melt extrusion is adopted to improve the dispersion uniformity of the material. Figure 1 to Figure 4 As shown, the melt premixing device includes a bracket 1, a transverse outer cylinder 2, a push plate 3 circumferentially fixed on the annular inner wall of the outer cylinder 2, and a pair of dispersion discs 4 arranged in the outer cylinder 2. A transverse mounting frame 5 is fixedly connected to one side of the bracket 1. The mounting frame 5 extends into the outer cylinder 2 and one end of the outer cylinder 2 is rotatably connected to the mounting frame 5. The other end of the outer cylinder 2 is rotatably connected to the bracket 1 on the other side. A transverse driving shaft 6 is arranged in the mounting frame 5. The outer end of the driving shaft 6 is meshed and connected to the outer cylinder 2. A pair of dispersion discs 4 are distributed up and down. The dispersion discs 4 are vertically meshed and connected to the inner end of the driving shaft 6 through a rotating shaft 7. The rotating shaft 7 passes through the dispersion disc 4. A slider 8 is rotatably connected to the rotating shaft 7, and the slider 8 is circumferentially slidably connected to the inner wall of the outer cylinder 2. The rotation of the driving shaft 6 drives the outer cylinder 2 to rotate and drives the dispersion disc 4 to rotate, and the surface where the outer cylinder 2 rotates is perpendicular to the surface where the dispersion disc 4 rotates. The rotating shaft 7 is meshed and connected to the driving shaft 6 through a bevel gear assembly 62.
[0035] The pushing plates 3 are divided into two groups, each group of pushing plates 3 includes a plurality of pushing plates 3 evenly distributed around the circumference, and the two groups of pushing plates 3 are distributed on both sides of the rotating shaft 7 , so that the pushing plates 3 will not interfere with the rotating shaft 7 when rotating with the outer cylinder 2 .
[0036] The outer wall of one side of the outer cylinder 2 is connected with a sleeve 21, and the sleeve 21 is sleeved outside the mounting frame 5. The drive shaft 6 is fixed with an A gear 61, and the inner wall of the sleeve 21 is provided with a gear ring 22. The A gear 61 partially passes through the mounting frame 5 and meshes with the gear ring 22. The mounting frame 5 is a hollow structure, and the outer end of the drive shaft 6 is rotatably connected to the bracket 1, and the drive shaft 6 is driven to rotate by the motor 9. The outer cylinder 2 and the mounting frame 5 are connected through bearings and sealing rings.
[0037] A circular slide rail 23 is provided inside the outer cylinder 2 , and a pair of sliders 8 are slidably embedded in the slide rail 23 .
[0038] The longitudinal section of the dispersion disk 4 is arcuate, and the centers of a pair of dispersion disks 4 face the sliders 8 respectively; a plurality of scattering holes 41 are formed on the dispersion disk 4 .
[0039] When the improved melt premixing device of the present invention is working, the driving shaft 6 rotates to drive the outer cylinder 2 to rotate circumferentially on the vertical plane, so that the material in the outer cylinder 2 can be stirred, melted and mixed through the pushing plate 3. At the same time, the driving shaft 6 can drive the two rotating shafts 7 to rotate circumferentially on the horizontal plane, so that the material in the outer cylinder 2 can be stirred, melted and mixed through the dispersion disk 4. At the same time, when the pushing plate 3 rotates with the outer cylinder 2, it can also drive the material to rotate and fall onto the dispersion disk 4, and disperse and fall through the dispersion disk 4, further promoting melt mixing.
[0040] The single stirring melt premixing device in the prior art was used to prepare antistatic double-layer composite wire tubes according to the methods of Examples 1-5, namely Comparative Examples 1-5. The results showed that the surface resistance of the composite wire tubes decreased by 4.33%, 4.18%, 4.21%, 4.32%, and 4.26%, respectively, and the tensile strength loss rate after aging in an oven at 100° C. for 100 hours increased by 6.14%, 6.22%, 6.21%, 6.17%, and 6.19%, respectively.
[0041] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an antistatic double-layer composite wire tube, characterized in that: The following steps are involved: (a) PVC resin, conductive carbon black, ABS resin, and SAN-b-PVC compatibilizer are prepared in proportion as the raw materials for the inner layer; PVC resin, 2,6-di-tert-butyl-4-allylphenol, diisopropylbenzene peroxide, and ASA resin are prepared in proportion and mixed evenly as the raw materials for the outer layer; (b) melt premixing the inner layer raw material and the outer layer raw material respectively by using a melt premixing device; (c) respectively inputting the two pre-melts of step (b) into a screw extruder, and extruding and molding by a double-layer co-extrusion method, and obtaining an antistatic double-layer composite wire tube after cooling and molding; The melt premixing device comprises a support (1), a transverse outer cylinder (2), a push plate (3) circumferentially distributed and fixedly mounted on the annular inner wall of the outer cylinder (2), and a pair of dispersion plates (4) arranged in the outer cylinder (2), wherein one side of the support (1) is fixedly connected with a transverse mounting frame (5), the mounting frame (5) extends into the outer cylinder (2) and one end of the outer cylinder (2) is rotatably connected to the mounting frame (5), and the other end of the outer cylinder (2) is rotatably connected to the support (1) on the other side, and a transverse drive shaft (6) is arranged in the mounting frame (5), and the drive shaft (6) ) is meshed and transmission-connected with the outer cylinder (2); a pair of dispersion discs (4) are distributed up and down; the dispersion discs (4) are vertically meshed and transmission-connected with the inner end of the drive shaft (6) via a rotating shaft (7); the rotating shaft (7) passes through the dispersion discs (4); a slider (8) is rotatably connected to the rotating shaft (7); and the slider (8) is circumferentially slidably connected to the inner wall of the outer cylinder (2); the rotation of the drive shaft (6) drives the outer cylinder (2) to rotate and drives the dispersion discs (4) to rotate; and the surface on which the outer cylinder (2) rotates is perpendicular to the surface on which the dispersion discs (4) rotate.
2. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: In step (a), based on 100% of the total mass of the inner layer raw materials, the inner layer raw materials include 62.4-68.5% of PVC resin, 7.5-10% of conductive carbon black, 17-21.5% of ABS resin, and 6.5-8.6% of SAN-b-PVC compatibilizer.
3. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: In step (a), based on 100% of the total mass of the outer layer raw materials, the outer layer raw materials include 79.6-81.15% of PVC resin, 0.2-0.3% of 2,6-di-tert-butyl-4-allyl phenol, 0.1-0.2% of diisopropylbenzene peroxide, and 16.4-20% of ASA resin.
4. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: In step (b), the temperature of the melt premixing of the inner layer raw material and the outer layer raw material is 165-170°C.
5. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: During the extrusion of the inner layer raw material in step (c), the temperatures of zones 1 to 5 of the extruder are 160-165°C, 165-170°C, 170-175°C, 175-180°C, and 180-185°C, respectively.
6. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: During the extrusion of the outer layer raw material in step (c), the temperatures of zones 1 to 5 of the extruder are 160-164°C, 164-170°C, 170-175°C, 175-180°C, and 180-185°C, respectively.
7. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: During double-layer co-extrusion, the co-extrusion die temperature is controlled at 185°C.
8. The method for preparing an antistatic double-layer composite wire tube according to claim 1, characterized in that: The cooling molding temperature is 20-30℃.
Citation Information
Patent Citations
Double-Color Double-Wall Corrugated Pipe and Preparation Method Therefor
AU2020102713A4
Method for preparing modified acrylonitrile-bivinyl-styrene copolymer
CN102838711A
Method for preparing antistatic extrusion hard PVC pipe raw materials for coal mine
CN106519476A
High-performance polyamide-based dyeable conductive fiber and preparation method thereof
CN106757507A
Toughened aging-resistant polyolefin composition and preparation method thereof
CN111040303A