Method for foaming and forming thermoplastic sheet and related device and formed foamed thermoplastic sheet
Through the double-plate/soft connection module forming method with supercritical carbon dioxide foaming and flexible connector adjustment, the molding problem of thermoplastics with high glass transition temperature is solved, and foamed sheets of uniform thickness and density are achieved, and cracking and The surface is wrinkled.
Patent Information
- Application Number
- CN202280048536.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-09
- Filing Date
- 2022-05-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-05-27
AI Technical Summary
The prior art is difficult to effectively deal with the foaming and forming of thermoplastics with high glass transition temperatures, which can easily lead to cracking, surface deformation and uneven foamed sheet thickness and density.
The cooling and forming method of double-plate/soft connection modules adjusted by supercritical carbon dioxide foaming combined with flexible connectors is adopted. The metal plates with multiple grooves are pressed and formed, and the control panels are spaced to prevent cracking and surface wrinkles, and uniform thickness is achieved. and density.
The cracking and surface deformation of thermoplastics at high glass transition temperatures is successfully avoided, ensuring the uniform thickness and density of foamed sheets, and improving the forming quality.
Smart Images

Figure CN117615894B_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims the benefit of EP application number 21184715.7 filed on July 9, 2021, which is incorporated herein by reference in its entirety. Background Art
[0003] Foaming thermoplastics with supercritical carbon dioxide is a cost-effective and residue-free method for forming foamed thermoplastic sheets. Commercially, a combination of a foaming step and a subsequent shaping step is mainly performed on thermoplastics with a glass transition temperature of less than 0°C (including polypropylene, thermoplastic polyurethane, ethylene-vinyl acetate copolymers and polyester elastomers). Typically, foaming is performed in a high-temperature foaming machine and then the foamed sheet is transferred to a separate room temperature cooling shaping machine. This method works for thermoplastics with a glass transition temperature of less than 0°C because they are still soft when the foamed sheet is transferred to the room temperature cooling shaping machine. However, the application of this two-step method to thermoplastics with higher glass transition temperatures is problematic because the foamed sheet is prone to cracking, surface deformation, and uneven foamed sheet thickness and density. Therefore, there is a need for an improved cooling shaping method for preparing foamed sheets from thermoplastics with a glass transition temperature of at least 20°C using supercritical carbon dioxide. Summary of the invention
[0004] One embodiment is a method of foaming and forming a thermoplastic sheet, comprising: foaming a thermoplastic sheet with supercritical carbon dioxide to form a foamed thermoplastic sheet, wherein the thermoplastic sheet comprises a thermoplastic composition comprising poly(phenylene ether), polyetherimide, or a combination thereof, and wherein the thermoplastic composition is characterized by a thermal conductivity of 100% to 50% according to ASTM D 1478. D3418-15 has a glass transition temperature of 20 to 300°C as determined by differential scanning calorimetry at a heating rate of 20°C / minute; and forming the foamed thermoplastic sheet to form a shaped foamed thermoplastic sheet, wherein the forming includes pressing the foamed thermoplastic sheet between a first metal plate and a second metal plate, wherein a surface of the first metal plate and a surface of the second metal plate include a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm; wherein the first metal plate and the second metal plate are connected by a flexible linkage capable of adjusting a separation between the first metal plate and the second metal plate; and wherein pressing the foamed thermoplastic sheet between the first metal plate and the second metal plate includes controlling a minimum separation between the first metal plate and the second metal plate.
[0005] Another embodiment is a shaped foamed thermoplastic sheet produced by the method described herein in any variation thereof and comprising a plurality of projections corresponding to a plurality of grooves of a first metal sheet and a second metal sheet.
[0006] Another embodiment is an electric vehicle battery comprising the shaped foamed thermoplastic sheet in any variation thereof.
[0007] Another embodiment is an apparatus for forming a foamed thermoplastic sheet, comprising: a first metal plate and a second metal plate, wherein the first metal plate and the second metal plate each include a major surface facing the thermoplastic plastic, wherein the major surface facing the thermoplastic plastic of the first metal plate or the second metal plate or both includes a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and wherein the major surface facing the thermoplastic plastic of the first metal plate or the second metal plate or both includes a rigid spacer to control a minimum spacing between the first metal plate and the second metal plate; a flexible connector connecting the first metal plate and the second metal plate, the flexible connector capable of adjusting the spacing between the first metal plate and the second metal plate; and a hydraulic system capable of pressing the flexible connector connecting the first metal plate and the second metal plate.
[0008] These and other embodiments are described in detail below. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In the drawings, like elements are similarly numbered throughout the several views.
[0010] Figure 1 is a schematic diagram of the first metal plate 160 and the second metal plate 170 ; the inserted figure is an enlarged cross-sectional view of a portion of the second metal plate 170 .
[0011] Figure 2 is a schematic diagram of a method for foaming and forming a thermoplastic sheet according to the present invention.
[0012] Figure 3 is a schematic diagram of a comparative method of foaming and forming a thermoplastic sheet without using the first and second metal plates or the flexible connector connecting the first and second metal plates of the present invention.
[0013] Figure 4 is a schematic diagram of a comparative method of foaming and forming a thermoplastic sheet without the use of the flexible connector of the present invention connecting the first and second metal sheets. DETAILED DESCRIPTION
[0014] The present inventors have determined that thermoplastics having a glass transition temperature of at least 20°C can be foamed with supercritical carbon dioxide and then cooled and formed by a method including cooling and forming steps utilizing grooved metal sheets connected by flexible connectors without producing cracking, surface deformation, uneven foamed sheet thickness, or uneven foamed sheet density.
[0015] Thus, one embodiment is a method of foaming and forming a thermoplastic sheet, comprising: foaming a thermoplastic sheet with supercritical carbon dioxide to form a foamed thermoplastic sheet, wherein the thermoplastic sheet comprises a thermoplastic composition comprising poly(phenylene ether), polyetherimide, or a combination thereof, and wherein the thermoplastic composition is characterized by a glass transition temperature of 20 to 300° C. as measured by differential scanning calorimetry at a heating rate of 20° C. / min according to ASTM D3418-15; and forming the foamed thermoplastic sheet to form a shaped foamed thermoplastic sheet, wherein the forming comprises forming the foamed thermoplastic sheet The foamed thermoplastic sheet is pressed between a first metal plate and a second metal plate, wherein a surface of the first metal plate and a surface of the second metal plate include a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm, wherein the first metal plate and the second metal plate are connected by a flexible connector capable of adjusting the spacing between the first metal plate and the second metal plate, and wherein pressing the foamed thermoplastic sheet between the first metal plate and the second metal plate includes controlling a minimum spacing between the first metal plate and the second metal plate.
[0016] The first metal plate, the second metal plate and the flexible connector form a double plate / soft connection module together. The flexible connector allows the double plate / soft connection module to be pressed, thereby adjusting the interval between the first metal plate and the second metal plate. When the double plate / soft connection module is not pressed, the interval between the first metal plate and the second metal plate makes the first (upper) metal plate not in contact with the shaped foamed thermoplastic sheet. When the double plate / soft connection module is pressed, the interval between the first metal plate and the second metal plate makes the first (upper) metal plate and the second (lower) metal plate both in contact with the shaped foamed thermoplastic sheet. The minimum interval between the first metal plate and the second metal plate is controlled by one or more rigid spacers attached to the surface of the first metal plate, the second metal plate or both facing the thermoplastic.
[0017] In some embodiments of the method, the flexible connector comprises a metal wire, a metal strip, a poly(p-phenylene terephthalamide) fiber, a carbon fiber, a glass fiber, or a combination thereof. In some embodiments of the method, the flexible connector comprises a metal wire, a metal strip, or a combination thereof. In some embodiments, the flexible connector comprises a metal wire or a metal strip comprising galvanized iron, the galvanized iron comprising 99.9 to 99.99 weight percent iron and 0.01 to 0.1 weight percent carbon based on the weight of the galvanized iron.
[0018] The main surface of the first metal plate and the second metal plate facing the thermoplastic includes a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm. Within these ranges, the width can be 0.2 to 1 mm, the depth can be 0.2 to 1 mm, and the center-to-center groove spacing can be 1 to 5 mm. In some embodiments, the metal plate surface includes a plurality of parallel grooves. In some embodiments, the metal plate surface includes a first group of parallel grooves and a second group of parallel grooves, wherein the first group of grooves is perpendicular to the second group of grooves.
[0019] In some embodiments, foaming the thermoplastic sheet with supercritical carbon dioxide to form a foamed thermoplastic sheet includes exhausting the carbon dioxide from a foaming machine in 10 seconds or less, or 5 seconds or less, or 3 seconds or less.
[0020] The thermoplastic composition is characterized by a glass transition temperature of 20 to 300°C as determined by differential scanning calorimetry according to ASTM D3418-15 at a heating rate of 20°C / minute. Within this range, the glass transition temperature may be 50 to 300°C or 100 to 300°C or 120 to 300°C.
[0021] In some embodiments of the method, the thermoplastic composition comprises poly(phenylene ether). For example, based on the total weight of the thermoplastic composition, the thermoplastic composition can comprise 40 to 78 weight percent of poly(phenylene ether); 10 to 48 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, wherein the sum of the weight percents of poly(phenylene ether), polystyrene or rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent. As another example, the thermoplastic composition can include 50 to 78 weight percent of poly(phenylene ether); 10 to 38 weight percent of polystyrene, rubber modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, based on the total weight of the thermoplastic composition, wherein the sum of the weight percents of the poly(phenylene ether), polystyrene or rubber modified polystyrene or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
[0022] In some embodiments of the method, the thermoplastic composition comprises a polyetherimide.
[0023] Another embodiment is a shaped foamed thermoplastic sheet produced by any of the above method embodiments and comprising a plurality of protrusions on both major surfaces thereof, the plurality of protrusions corresponding to the plurality of grooves of the first metal sheet and the second metal sheet.
[0024] Another embodiment is a shaped foamed thermoplastic sheet produced by a variation of any of the above methods and comprising poly(phenylene ether). For example, the thermoplastic composition can comprise 40 to 78 weight percent poly(phenylene ether); 10 to 48 weight percent polystyrene, rubber-modified polystyrene, or a combination thereof; 2 to 10 weight percent block copolymers comprising polystyrene blocks and polybutadiene blocks, block copolymers comprising polystyrene blocks and hydrogenated polybutadiene blocks, or a combination thereof; and 10 to 20 weight percent flame retardant, wherein the sum of the weight percents of poly(phenylene ether), polystyrene or rubber-modified polystyrene, or a combination thereof, block copolymers, and flame retardant is 95 to 100 weight percent, based on the total weight of the thermoplastic composition. As another example, the thermoplastic composition can include 50 to 78 weight percent of poly(phenylene ether); 10 to 38 weight percent of polystyrene, rubber modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, based on the total weight of the thermoplastic composition, wherein the sum of the weight percents of the poly(phenylene ether), polystyrene or rubber modified polystyrene or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
[0025] Another embodiment is a shaped foamed thermoplastic sheet produced by any variation of the above method and comprising a polyetherimide.
[0026] Another embodiment is an electric vehicle battery comprising the shaped foamed thermoplastic sheet in any of the above variations thereof.
[0027] Another embodiment is an apparatus for forming a foamed thermoplastic sheet, comprising: a first metal plate and a second metal plate, wherein the first metal plate and the second metal plate each include a major surface facing the thermoplastic, wherein the major surfaces of the first metal plate and the second metal plate facing the thermoplastic include a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm, and wherein the major surfaces of the first metal plate or the second metal plate or both facing the thermoplastic include rigid spacers to control a minimum spacing of the first metal plate and the second metal plate; a flexible connector connecting the first metal plate and the second metal plate, the flexible connector being capable of adjusting the spacing between the first metal plate and the second metal plate; and a hydraulic system capable of pressing the flexible connector connecting the first metal plate and the second metal plate. Figure 1is a schematic diagram of a first metal plate 160 and a second metal plate 170, each of which includes a perforation 161. The surface of the second metal plate 170 facing the thermoplastic includes a groove 174 and includes two rigid spacers 175 to control the minimum spacing of the first metal plate 160 from the second metal plate 170. Figure 1 The inset in is an enlarged cross-sectional view of a portion of the second metal plate 170 and illustrates the groove width 171 , the groove depth 172 , and the center-to-center groove spacing 173 .
[0028] In some embodiments of the device, the flexible connector comprises a metal wire, a metal strip, poly(p-phenylene terephthalamide) fiber, a carbon fiber, a glass fiber, or a combination thereof. In some embodiments of the method, the flexible connector comprises a metal wire, a metal strip, or a combination thereof. In some embodiments, the flexible connector comprises a metal wire or a metal strip comprising galvanized iron, wherein the galvanized iron comprises 99.9 to 99.99 weight percent iron and 0.01 to 0.1 weight percent carbon based on the weight of the galvanized iron.
[0029] All ranges disclosed herein are inclusive of the endpoints, and the endpoints are independently combinable with each other. Each range disclosed herein constitutes a disclosure of any point or sub-range within the disclosed range.
[0030] The present invention is further illustrated by the following non-limiting examples.
[0031] Example
[0032] The components used for these experiments are summarized in Table 1.
[0033] Table 1
[0034]
[0035] The resin compositions are summarized in Table 2, where the component amounts are expressed as weight percent based on the total weight of the composition. The compositions were compounded on a 36 mm twin screw extruder operating at barrel temperatures of 200, 230, 260, 260, 280, 280, 280, 285 and 275°C from feed throat to die and a die temperature of 275°C. The extrudate was cooled and pelletized, then dried at 100°C for 3 hours before use for sheet extrusion. The glass transition temperature, expressed in degrees Celsius, was determined by differential scanning calorimetry according to ASTM D3418-15 at a heating rate of 20°C / min.
[0036] Table 2
[0037]
[0038]
[0039] Sheet extrusion of the resin composition was performed on a sheet extrusion apparatus operating at barrel temperatures of 200, 240, 260, 270, 280, 280, 260, 250° C. and a die temperature of 245° C. Sheet thickness is described below in the context of each experiment.
[0040] Example 1
[0041] This experiment utilizes the extruded sheet of resin A with 300 mm length, 200 mm width and 5 mm thickness. Also use two aluminum plates with 1000 mm length, 600 mm width and 5 mm thickness. The inner (facing thermoplastic) surface of two aluminum plates is machined to produce the vertical micro groove grid with 0.5 mm width, 0.5 mm depth and 2 mm center to center groove interval. By perforating the four corners of these aluminum plates and connecting these aluminum plates to the soft connector (connecting rod, link) to produce double plate / soft connection module, this soft connector is made up of the metal wire hoop with circular cross section, 1 mm wire cross section diameter and about 200 mm hoop circumference. The metal wire for forming the hoop is the galvanized iron wire containing 99.98 weight percent iron and 0.02 weight percent carbon. The connection of aluminum plate to the wire hoop is realized by repeatedly looping the wire of the wire hoop through each hole in the aluminum plate. In the double plate / soft joint module, the initial spacing between the two aluminum plates is about 25 mm, but the spacing can be reduced by pressing the double plate / soft joint module to produce a minimum plate spacing equal to or slightly less than (e.g., about 5% less) the thickness of the final foamed sheet. The minimum plate spacing is controlled by two rigid spacers attached to the opposite edges of the surface of the lower aluminum plate facing the thermoplastic.
[0042] The extruded sheet is placed between two aluminum plates separated by about 25 mm. The cavity of the foaming machine is preheated to 160°C, and then the double plate / soft connection module containing the extruded sheet is placed in the foaming machine 1, and the mold cavity is closed by the hydraulic press of the foaming machine. The closure of the mold cavity does not affect the plate spacing of about 25 mm. Then, supercritical carbon dioxide is injected into the cavity of the foaming machine, and the temperature of 160°C and the carbon dioxide pressure of 20 MPa are maintained for 60 minutes.
[0043] After 60 minutes have passed, the pressure is released through the exhaust port in about 2 seconds, and the cavity is opened. At this point, the foamed sheet has a warped (ie, non-flat) shape. The double plate / soft connection module containing the foamed sheet is quickly transferred to a forming machine, which has an initial temperature of about 23°C, and the hydraulic press of the forming machine is quickly closed, resulting in a plate spacing of 21 mm and a pressure of about 0.6 MPa. Five minutes later, the hydraulic press increases the plate spacing to about 25 mm, and the foamed sheet is removed from the double plate / soft connection module. The resulting flat formed foamed sheet has a thickness of 21 mm and a density of 0.045 g / cm3 measured according to ASTM D1622-14. The main surface of the sheet includes a protrusion corresponding to the groove in the aluminum plate. The formed foamed sheet does not show cracking or surface wrinkling, and its thickness and density are uniform.
[0044] Figure 2 1 is a schematic diagram of a method for foaming and forming a thermoplastic sheet according to the present invention and Example 1. The method uses a foaming machine 10 and a forming machine. Figure 2 , the forming machine is shown in an unpressed configuration 20 and a pressed configuration 30. The foaming machine 10 includes a foaming machine upper hydraulic press 110 and a foaming machine lower hydraulic press 120 that control vertical movement of the foaming machine upper wall 140 and the foaming machine lower wall 150, respectively. Embedded in the foaming machine upper wall 140 is a carbon dioxide inlet / outlet with a valve 130. Shown within the chamber of the foaming machine 10 is a dual plate / soft connection module, which includes a first metal plate 160 and a second metal plate 170 connected by a flexible connection 180. An unfoamed thermoplastic sheet 190 rests on the second metal plate 170. After the unfoamed thermoplastic sheet 190 is foamed with carbon dioxide to form a foamed unformed thermoplastic sheet 290 in the foaming machine 10, the carbon dioxide is discharged via the carbon dioxide inlet / outlet with a valve 130, and the chamber is opened via the foaming machine upper hydraulic press 110 and the foaming machine lower hydraulic press 120. The dual plate / soft connection module is quickly transferred from the foaming machine 10 to the forming machine in the unpressed configuration 20. The transfer is indicated by the arrow marked 200. The forming machine includes a forming machine upper hydraulic press 210, a forming machine lower hydraulic press 220, a forming machine upper hydraulic contact plate 230 and a forming machine lower hydraulic contact plate 240. The forming machine upper hydraulic press 210 and the forming machine lower hydraulic press 220 are used to convert the forming machine from its unpressed configuration 20 to its pressed configuration 30, wherein the minimum spacing of the first metal plate 160 and the second metal plate 170 is formed by at least one rigid spacer 175 ( Figure 2 Not shown, but in Figure 1The forming machine is controlled by the forming machine (shown in FIG). The conversion of the forming machine from its unpressed configuration to its pressed configuration is indicated by the arrow marked 300. In the pressed configuration 30 of the forming machine, the foamed unformed thermoplastic sheet is formed and cooled to form a flawless formed foamed sheet 390. Then, the forming machine is converted back to its unpressed configuration 20 using the forming machine upper hydraulic press 210 and the forming machine lower hydraulic press 220, the double plate / soft connection module is removed from the forming machine, and the flawless formed foamed sheet 390 is removed from the double plate / soft connection module. The removal of the formed foamed sheet is indicated by the arrow marked 400.
[0045] Example 2
[0046] The procedure of Example 1 was followed, except that the spacing between the plates during foaming was about 17 mm, foaming was performed at 145°C, and the spacing between the plates during forming was about 10 mm. The resulting flat shaped foamed sheet had a thickness of about 10 mm and a density of 0.14 g / cm3 as determined according to ASTM D1622-14. The surface of the sheet included protrusions corresponding to the grooves in the aluminum plate. The shaped foamed sheet exhibited no cracking or surface wrinkling, and its thickness and density were uniform.
[0047] Example 3
[0048] The procedure of Example 1 was followed, except that Resin B was used, foaming was carried out at 165°C for 70 minutes, and the plate spacing during forming was about 19 mm. The resulting flat shaped foamed sheet had a thickness of about 19 mm and a density of 0.065 g / cm3 as determined according to ASTM D1622-14. The surface of the sheet included protrusions corresponding to the grooves in the aluminum plate. The shaped foamed sheet exhibited no cracking or surface wrinkling, and its thickness and density were uniform.
[0049] Example 4
[0050] The procedure of Example 1 was followed, except that the thermoplastic sheet had a thickness of 3 mm, the plate spacing during foaming was about 12 mm, foaming was performed at 145° C. for 50 minutes, and the plate spacing during forming was about 7 mm. The resulting flat foamed shaped sheet had a thickness of about 7 mm and a density of 0.15 g / cm3 as measured according to ASTM D1622-14. The surface of the sheet included protrusions corresponding to the grooves in the aluminum plate. The shaped foamed sheet exhibited no cracking or surface wrinkling, and its thickness and density were uniform.
[0051] Comparative Example 1
[0052] This experiment used an extruded sheet of resin A having a length of 300 mm, a width of 200 mm, and a thickness of 5 mm. No aluminum plate was used in this experiment.
[0053] The extruded sheet was placed on the lower surface of the hydraulic press of the foaming machine cavity which had been preheated to 160°C. The mold cavity of the foaming machine was closed by the hydraulic system, creating a gap of about 50 mm between the upper and lower surfaces of the hydraulic press. Then, supercritical carbon dioxide was injected into the cavity of the foaming machine, and a temperature of 160°C and a carbon dioxide pressure of 20 MPa were maintained for 60 minutes.
[0054] After 60 minutes have passed, the pressure is released through the exhaust port and the cavity is opened. At this point, the foamed sheet has a warped (i.e., non-flat) shape. The foamed sheet is quickly transferred to a forming machine having an initial temperature of about 23°C, and the hydraulic press of the forming machine is quickly closed, creating a gap of about 20 mm between the upper and lower surfaces of the hydraulic press, and a pressure of about 0.6 MPa. After 5 minutes, the gap between the upper and lower surfaces of the hydraulic press is increased to about 200 mm, and the formed foamed sheet is removed from the forming machine. The thickness of the resulting formed foamed sheet is about 20 mm, and the density measured according to ASTMD1622-14 is 0.045 g / cm3, but it exhibits unacceptable cracking, and the surface of the foamed sheet exhibits unacceptable surface wrinkling.
[0055] exist Figure 3 The process is schematically shown in Figure 2 Similar, except that the dual panel / flexible connection module is not used and the final product is a formed foam sheet 394 that exhibits cracking and surface wrinkling.
[0056] Comparative Example 2
[0057] This experiment uses the extruded sheet of resin A with 300 mm length, 200 mm width and 5 mm thickness. Also use two aluminum plates with 1000 mm length, 600 mm width and 5 mm thickness. The inner surface of the two aluminum plates is machined to produce a vertical micro-groove grid with a width of 0.5 mm, a depth of 0.5 mm and a center-to-center groove spacing of 2 mm. Bolt the aluminum plates to produce a fixed spacing of about 20 mm, thereby producing a double plate / fixed spacing module.
[0058] The extruded sheet was placed between two aluminum plates. The cavity of the foaming machine was heated to 160°C, and then the double plate / fixed spacer module containing the extruded sheet was placed in the foaming machine, and the mold cavity was closed. Then, supercritical carbon dioxide was injected into the cavity of the foaming machine, and the temperature of 160°C and the carbon dioxide pressure of 20 MPa were maintained for 60 minutes.
[0059] After 60 minutes have passed, the pressure is released through the exhaust port and the cavity is opened. At this point, the foamed sheet has a warped (i.e., non-flat) shape. The double plate / fixed spacing module containing the foamed sheet is quickly transferred to a forming machine with an initial temperature of about 23°C. The plate spacing is still fixed at about 20 mm. After 5 minutes, the foamed sheet is removed from the double plate / fixed spacing module. Figure 3 The process is schematically shown in FIG. The resulting shaped foam sheet had a thickness of about 20 mm and a density of 0.045 g / cm 3 , but the surface of the foamed sheet exhibited unacceptable surface wrinkling, and the thickness and density were not uniform throughout the sheet.
[0060] exist Figure 4 The process is schematically shown in Figure 2 Similar, except that a double plate / fixed spacing module is used instead of a double plate / soft connection module, in which a rigid spacer 185 connects the first metal plate 160 and the second metal plate 170 and creates a fixed spacing between the first metal plate 160 and the second metal plate 170, and the final product is a formed foam sheet 396 exhibiting surface wrinkling and uneven thickness and density.
[0061] Comparative Example 3
[0062] The experiment used an extruded sheet of resin A with a length of 300 mm, a width of 200 mm and a thickness of 5 mm. Two aluminum plates with a length of 1000 mm, a width of 600 mm and a thickness of 5 mm were also used. None of the aluminum plates had grooves. A double plate / soft connection module was produced by perforating the four corners of the aluminum plate and connecting the aluminum plate to a soft connection piece, which consisted of a metal wire hoop with a circular cross-section, a wire section diameter of 1 mm and a hoop circumference of about 200 mm. The initial spacing between the two aluminum plates was about 25 mm, but the spacing could be reduced by pressing the double plate / soft connection module to produce a plate spacing equal to or slightly less than (e.g., almost 5% smaller) the thickness of the final foamed sheet.
[0063] The extruded sheet is placed between two aluminum plates. The cavity of the foaming machine is heated to 160°C, and then the double plate / soft connection module containing the extruded sheet is placed in the foaming machine, and the mold cavity is closed. The closure of the mold cavity does not affect the plate spacing of about 25 mm. Then, supercritical carbon dioxide is injected into the cavity of the foaming machine, and the temperature of 160°C and the carbon dioxide pressure of 20 MPa are maintained for 60 minutes.
[0064] After 60 minutes have passed, the pressure is released through the exhaust port and the cavity is opened. At this point, the foamed sheet has a warped (ie, non-flat) shape. The double plate / soft connection module containing the warped foamed sheet is quickly transferred to a forming machine with an initial temperature of about 23°C. The hydraulic press of the forming machine is quickly closed, resulting in a plate spacing of about 7 mm and a pressure of about 0.6 MPa. After 5 minutes, the shaped foamed sheet is removed from the double plate / soft connection module. The resulting shaped foamed sheet has a thickness of about 7 mm and a density of 0.15 g / cm3, but the thickness and density are uneven throughout the sheet.
[0065] This process is similar to Figure 2 The process schematically shown in FIG. 1 is similar to that in FIG. 1 , except that the first metal plate 160 and the second metal plate 170 do not have grooves.
[0066] Table 3 summarizes the conditions and results of the above experiments. In Table 3, "N / A" means not applicable. Examples 1-4 were carried out according to the method of the present invention and used a double plate / soft connection module, in which both plates had grooved surfaces facing the thermoplastic sheet. The resulting shaped foamed sheet exhibited uniform thickness and density, and no cracking and surface wrinkling. In Comparative Example 1, the double plate / soft connection module was not used, and during forming, the foamed sheet was in direct contact with the smooth surface of the hydraulic press. The resulting shaped foamed sheet exhibited cracking and surface wrinkling. In Comparative Example 2, the grooved aluminum plate was maintained at a fixed interval of 20 mm during foaming and forming, and the resulting shaped foamed sheet exhibited surface wrinkling and uneven thickness and density. In Comparative Example 3, the aluminum plate had no grooves, and the resulting shaped foamed sheet exhibited uneven thickness and density.
[0067] Table 3
[0068]
[0069] Table 3 (continued)
[0070]
[0071]
[0072] The present invention includes at least the following aspects.
[0073] Aspect 1: A method of foaming and forming a thermoplastic sheet, comprising: foaming a thermoplastic sheet with supercritical carbon dioxide to form a foamed thermoplastic sheet, wherein the thermoplastic sheet comprises a thermoplastic composition comprising poly(phenylene ether), polyetherimide, or a combination thereof, and wherein the thermoplastic composition is characterized by a thermal conductivity of 100% by weight according to ASTM D 1478. D3418-15 has a glass transition temperature of 20 to 300°C as determined by differential scanning calorimetry at a heating rate of 20°C / minute; and forming the foamed thermoplastic sheet to form a shaped foamed thermoplastic sheet, wherein the forming comprises pressing the foamed thermoplastic sheet between a first metal plate and a second metal plate, wherein a surface of the first metal plate and a surface of the second metal plate include a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm, wherein the first metal plate and the second metal plate are connected by a flexible connector capable of adjusting the separation between the first metal plate and the second metal plate, and wherein pressing the foamed thermoplastic sheet between the first metal plate and the second metal plate includes controlling a minimum separation between the first metal plate and the second metal plate.
[0074] Aspect 2: The method according to aspect 1, wherein the flexible connector comprises a metal wire, a metal ribbon, poly(p-phenylene terephthalamide) fiber, a carbon fiber, a glass fiber, or a combination thereof.
[0075] Aspect 3: The method according to aspect 1 or 2, wherein the flexible connector comprises a metal wire or a metal strip comprising galvanized iron, wherein the galvanized iron comprises 99.9 to 99.99 weight percent iron and 0.01 to 0.1 weight percent carbon based on the weight of the galvanized iron.
[0076] Aspect 4: The method according to any of aspects 1-3, wherein the thermoplastic composition comprises poly(phenylene ether).
[0077] Aspect 5: The method according to aspect 4, wherein the thermoplastic composition has a glass transition temperature of 100 to 300°C and comprises, based on the total weight of the thermoplastic composition, 40 to 78 weight percent of the poly(phenylene ether); 10 to 48 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, wherein the sum of the weight percents of the poly(phenylene ether), the polystyrene or the rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
[0078] Aspect 6: The method according to aspect 4, wherein the thermoplastic composition has a glass transition temperature of 100 to 300°C and comprises, based on the total weight of the thermoplastic composition, 50 to 78 weight percent of the poly(phenylene ether); 10 to 38 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, wherein the sum of the weight percents of the poly(phenylene ether), the polystyrene or the rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
[0079] Aspect 7: The method according to any of aspects 1-3, wherein the thermoplastic composition comprises a polyetherimide.
[0080] Aspect 8: A shaped foamed thermoplastic sheet produced by the method of any one of aspects 1 to 7, and comprising a plurality of protrusions corresponding to the plurality of grooves of the first metal plate and the second metal plate.
[0081] Aspect 9: The shaped foamed thermoplastic sheet according to aspect 8, wherein the thermoplastic composition comprises poly(phenylene ether).
[0082] Aspect 10: A shaped foamed thermoplastic sheet according to Aspect 9, wherein the thermoplastic composition has a glass transition temperature of 100 to 300°C and comprises, based on the total weight of the thermoplastic composition, 40 to 78 weight percent of the poly(phenylene ether); 10 to 48 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, wherein the sum of the weight percents of the poly(phenylene ether), the polystyrene or the rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
[0083] Aspect 11: A shaped foamed thermoplastic sheet according to Aspect 9, wherein the thermoplastic composition has a glass transition temperature of 100 to 300°C and comprises, based on the total weight of the thermoplastic composition, 50 to 78 weight percent of the poly(phenylene ether); 10 to 38 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof; 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof; and 10 to 20 weight percent of a flame retardant, wherein the sum of the weight percents of the poly(phenylene ether), the polystyrene or the rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
[0084] Aspect 12: The shaped foamed thermoplastic sheet according to Aspect 8, wherein the thermoplastic composition comprises a polyetherimide.
[0085] Aspect 13: An electric vehicle battery comprising the shaped foamed thermoplastic sheet of any one of aspects 8-12.
[0086] Aspect 14: An apparatus for forming a foamed thermoplastic sheet, comprising: a first metal plate and a second metal plate, wherein the first metal plate and the second metal plate each include a major surface facing the thermoplastic, wherein the major surfaces of the first metal plate and the second metal plate facing the thermoplastic include a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm, and wherein the major surfaces of the first metal plate or the second metal plate or both facing the thermoplastic include rigid spacers to control a minimum spacing between the first metal plate and the second metal plate; a flexible connector connecting the first metal plate and the second metal plate, the flexible connector being capable of adjusting the spacing between the first metal plate and the second metal plate; and a hydraulic system capable of pressing the flexible connector connecting the first metal plate and the second metal plate.
[0087] Aspect 15: The device according to aspect 14, wherein the flexible connector comprises a metal wire, a metal ribbon, poly(p-phenylene terephthalamide) fiber, a carbon fiber, a glass fiber, or a combination thereof.
Claims
1. A method for foaming and forming a thermoplastic sheet, comprising: foaming a thermoplastic sheet with supercritical carbon dioxide to form a foamed thermoplastic sheet, wherein the thermoplastic sheet comprises a thermoplastic composition comprising polyphenylene ether, polyetherimide, or a combination thereof, and wherein the thermoplastic composition is characterized by a glass transition temperature of 20 to 300°C as determined by differential scanning calorimetry at a heating rate of 20°C / minute according to ASTM D3418-15; and The foamed thermoplastic sheet is formed to form a shaped foamed thermoplastic sheet, wherein the forming includes pressing the foamed thermoplastic sheet between a first metal plate and a second metal plate, wherein a surface of the first metal plate and a surface of the second metal plate include a plurality of grooves, each groove having a width of 0.1 to 1 mm and a depth of 0.1 to 1 mm, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 mm, wherein the first metal plate and the second metal plate are connected by a flexible connector capable of adjusting the spacing between the first metal plate and the second metal plate, and wherein pressing the foamed thermoplastic sheet between the first metal plate and the second metal plate includes controlling a minimum spacing between the first metal plate and the second metal plate. 2 . The method according to claim 1 , wherein the flexible connector comprises a metal wire, a metal ribbon, poly(p-phenylene terephthalamide) fiber, a carbon fiber, a glass fiber, or a combination thereof.
3. The method according to claim 1 or 2, wherein the flexible connector comprises a metal wire or a metal strip comprising galvanized iron, wherein the galvanized iron comprises 99.9 to 99.99 weight percent of iron and 0.01 to 0.1 weight percent of carbon based on the weight of the galvanized iron.
4. The method of any one of claims 1-3, wherein the thermoplastic composition comprises polyphenylene ether.
5. The method according to claim 4, wherein the thermoplastic composition has a glass transition temperature of 100 to 300° C.; and based on the total weight of the thermoplastic composition, the thermoplastic composition comprises 40 to 78 weight percent of the polyphenylene ether, 10 to 48 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof, 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof, and 10 to 20 weight percent of a flame retardant; wherein the sum of the weight percents of the polyphenylene ether, the polystyrene or the rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
6. The method according to claim 4, wherein the thermoplastic composition has a glass transition temperature of 100 to 300° C.; and based on the total weight of the thermoplastic composition, the thermoplastic composition comprises 50 to 78 weight percent of the polyphenylene ether, 10 to 38 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof, 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof, and 10 to 20 weight percent of a flame retardant; wherein the sum of the weight percents of the polyphenylene ether, the polystyrene or rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
7. The method of any one of claims 1-3, wherein the thermoplastic composition comprises a polyetherimide.
8. A shaped foamed thermoplastic sheet produced by the method of any one of claims 1 to 7 and comprising a plurality of protrusions corresponding to the plurality of grooves of the first metal plate and the second metal plate.
9. The shaped foamed thermoplastic sheet of claim 8, wherein the thermoplastic composition comprises polyphenylene ether.
10. The shaped foamed thermoplastic sheet according to claim 9, wherein the thermoplastic composition has a glass transition temperature of 100 to 300°C; and based on the total weight of the thermoplastic composition, the thermoplastic composition comprises 40 to 78 weight percent of the polyphenylene ether, 10 to 48 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof, 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof, and 10 to 20 weight percent of a flame retardant; wherein the sum of the weight percents of the polyphenylene ether, the polystyrene or rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
11. The shaped foamed thermoplastic sheet according to claim 9, wherein the thermoplastic composition has a glass transition temperature of 100 to 300°C; and based on the total weight of the thermoplastic composition, the thermoplastic composition comprises 50 to 78 weight percent of the polyphenylene ether, 10 to 38 weight percent of polystyrene, rubber-modified polystyrene, or a combination thereof, 2 to 10 weight percent of a block copolymer comprising a polystyrene block and a polybutadiene block, a block copolymer comprising a polystyrene block and a hydrogenated polybutadiene block, or a combination thereof, and 10 to 20 weight percent of a flame retardant; wherein the sum of the weight percents of the polyphenylene ether, the polystyrene or rubber-modified polystyrene, or a combination thereof, the block copolymer, and the flame retardant is 95 to 100 weight percent.
12. The shaped foamed thermoplastic sheet of claim 8, wherein the thermoplastic composition comprises a polyetherimide.
13. An electric vehicle battery comprising the shaped foamed thermoplastic sheet according to any one of claims 8 to 12.
14. An apparatus for forming a foamed thermoplastic sheet using the method of any one of claims 1 to 7, comprising: a first metal plate and a second metal plate, wherein the first metal plate and the second metal plate each include a major surface facing the thermoplastic, wherein the major surfaces facing the thermoplastic of the first metal plate and the second metal plate include a plurality of grooves, each groove having a width of 0.1 to 1 millimeter and a depth of 0.1 to 1 millimeter, and each groove is spaced apart from the nearest groove by a center-to-center distance of 0.5 to 5 millimeters, and wherein the major surfaces facing the thermoplastic of the first metal plate or the second metal plate or both include rigid spacers to control a minimum spacing of the first metal plate and the second metal plate; a flexible connector connecting the first metal plate and the second metal plate, wherein the flexible connector is capable of adjusting a gap between the first metal plate and the second metal plate; and a hydraulic system capable of pressing the flexible connection connecting the first metal plate and the second metal plate, wherein the foamed thermoplastic sheet comprises a thermoplastic composition comprising polyphenylene ether, polyetherimide or a combination thereof, and The thermoplastic composition is characterized by a glass transition temperature of 20 to 300°C as determined by differential scanning calorimetry according to ASTM D3418-15 at a heating rate of 20°C / minute.
15. The device of claim 14, wherein the flexible connector comprises a metal wire, a metal ribbon, poly(p-phenylene terephthalamide) fiber, a carbon fiber, a glass fiber, or a combination thereof.