Metal-doped SrTiO3 / TiO2 photocatalytic material and its preparation method and application
By doping SrTiO3/TiO3 with metal elements to form an S-type heterojunction structure, the problem of large amounts of formic acid added in the existing photocatalytic denitrification process is solved, the nitrate conversion rate and N2 selectivity are improved, and high efficiency is achieved. photocatalytic denitrification effect, and reduces material usage and subsequent processing complexity.
Patent Information
- Application Number
- CN202311634320.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-11-30
AI Technical Summary
The large amount of formic acid added in the existing photocatalytic denitrification process results in a low pH reaction system, which damages the life of the material and affects the subsequent treatment process. The adsorption capacity of NO3- is insufficient and cannot be effectively directly reduced on the surface of the material.
Using metal-doped SrTiO3/TiO2 S-type heterojunction photocatalytic materials, metal elements such as Fe, Cu, Ce, Ag or Pd are doped into the SrTiO3 lattice to form a coupling heterostructure with anatase TiO2. Reduce the usage of formic acid and catalyst, and improve the conversion rate of nitrate and N2 selectivity.
It has been achieved to improve the photocatalytic denitrification performance under the condition of a small amount of formic acid. Using 100-400mg/L photocatalytic material and 20-40mmol/L formic acid can achieve more than 95% NO3- conversion rate and N2 selectivity, extending the material longevity and simplified subsequent handling.
Smart Images

Figure CN117619374B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of photocatalytic materials and wastewater treatment, and specifically relates to metal-doped SrTiO3 / TiO2 photocatalytic materials and preparation methods and applications thereof. Background Art
[0002] With the continuous and rapid development of modern industry, a large number of nitrogen-containing chemical synthetic products are used (such as synthetic rubber, paints and coatings, resins, electronic components and plastics, etc.), thus generating a large amount of nitrogen-containing industrial wastewater (such as fertilizer wastewater, electroplating wastewater, leather wastewater, coking wastewater, etc.). If the nitrogen-containing compounds in this type of industrial wastewater are discharged into surface water bodies, it will cause the accumulation of nitrogen compounds in the water environment, leading to serious deterioration such as eutrophication of water bodies, and hypoxia in water bodies will cause the death of a large number of organisms. Nitrates can also be converted into nitrites or endocrine disruptors (nitroaromatic hydrocarbons) in the human body, leading to methylhemoglobinemia or carcinogenic risks.
[0003] Among the existing technologies, photocatalysis is an environmentally friendly and promising water denitrification technology. Under certain conditions, nitrate nitrogen can be converted into non-toxic N2, avoiding secondary pollution to the environment. Many composite photocatalytic materials have been developed for nitrate reduction, for example, Pd-Cu / TiO2, Ag2O / P25, Cu2O / TiO2 and CuInS2 / TiO2 are used for nitrate reduction. The denitrification reaction of nitrate requires a large reduction potential. Most heterojunction materials cannot effectively generate highly reducing photogenerated electrons and are not very effective for NO3 - The adsorption capacity is insufficient and NO3 cannot be directly reduced on the surface of the material. - , a large amount of vacancy scavenger needs to be added to the catalytic reduction system to meet the needs of the denitrification reaction.
[0004] Formic acid is widely used as the best hole scavenger. After formic acid is added to the photocatalytic system, it can be oxidized by the photogenerated holes generated in the valence band of the photocatalytic material to produce CO2 - , making NO3 - Can be directly reacted with CO2 in solution - The reaction converts to nitrogen. However, in order to achieve high conversion rate and high selectivity when reducing nitrates, most denitrification photocatalytic materials require a large amount of catalyst and formic acid. For example, the NH2-MIL-Fe / BiVO4 disclosed in the Chinese invention patent with the authorization announcement number CN113457745B is used in the nitrate reduction reaction. When treating a 100mgN / L nitrate aqueous solution, 1g / L catalyst and 40-80mmol / L formic acid need to be added to achieve a conversion rate higher than 94.6% and a N2 selectivity higher than 93.4.
[0005] The addition of a large amount of formic acid makes the pH value of the photocatalytic reduction reaction system strongly acidic (pH ≤ 2.5). The low pH reaction system will not only lead to a large amount of dissolution of metal ions in the photocatalytic material and reduce the service life of the material, but also increase the requirements of the reaction on the equipment. It will also affect the subsequent wastewater treatment process due to formic acid residues and other reasons, limiting the engineering application of photocatalytic denitrification.
[0006] Therefore, studying efficient photocatalytic denitrification materials with a small amount or even no hole scavenger is of great significance for the application of photocatalytic denitrification. Summary of the invention
[0007] 1. Problem to be solved
[0008] In view of the large amount of formic acid added in the existing photocatalytic denitrification process (nitrate reduction process) and its adverse consequences, this application provides a metal-doped SrTiO3 / TiO2 photocatalytic material and its preparation method and application. The metal-doped SrTiO3 / TiO2 photocatalytic material is a metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material, specifically a coupled heterostructure formed by metal doping into the SrTiO3 lattice and anatase TiO2. Applying it to the photocatalytic reduction of nitrate process can reduce the use of formic acid and photocatalytic materials, and improve the conversion rate of photocatalytic reduction of nitrate and N2 selectivity.
[0009] 2. Technical solution
[0010] In order to solve the above problems, the technical solutions adopted in this application are as follows:
[0011] The present application provides a metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2, wherein X is a metal element that makes the material surface Lewis acid after doping, and X is doped into the SrTiO3 lattice and forms a coupled heterostructure with anatase TiO2.
[0012] Furthermore, in the above-mentioned photocatalytic material X-SrTiO3 / TiO2, the molar ratio of TiO2 to Sr element is 1:(1 to 1.5).
[0013] Furthermore, in the above-mentioned photocatalytic material X-SrTiO3 / TiO2, the molar ratio of the metal element to the Sr element is 1:(10-200).
[0014] Furthermore, in the above-mentioned photocatalytic material X-SrTiO3 / TiO2, the metal elements include Fe element, Cu element, Ce element, Ag element or Pd element, and the corresponding photocatalytic materials are Fe-SrTiO3 / TiO2, Cu-SrTiO3 / TiO2, Ce-SrTiO3 / TiO2, Ag-SrTiO3 / TiO2 or Pd-SrTiO3 / TiO2.
[0015] Furthermore, in the above-mentioned photocatalytic material X-SrTiO3 / TiO2, the metal element includes Fe element or Cu element.
[0016] The present application also provides a method for preparing the above-mentioned metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2, which specifically comprises the following steps:
[0017] S1, preparation of X-doped SrTiO3, take an appropriate amount of ethanolamine aqueous solution in a container, slowly add tetrabutyl titanate to the ethanolamine under stirring at room temperature, stir for 10 minutes, add NaOH solution to the mixed solution, then transfer it to an ultrasonic tank, add strontium nitrate and X nitrate mixed aqueous solution, ultrasonically form a suspension, continue stirring for 30 minutes, transfer it to a high-pressure hydrothermal autoclave lined with tetrafluoroethylene, and heat it in an oven; after the hydrothermal autoclave is naturally cooled, separate the reaction precipitate, wash it repeatedly with ethanol and deionized water, put it in a vacuum drying oven, and dry it to obtain X-SrTiO3 powder; strontium nitrate and X nitrate are simultaneously added to the strongly alkaline ethanolamine and tetrabutyl titanate mixed solution, and stirred rapidly, the purpose is to make the element X and the Sr element react simultaneously and dope with each other, so as to facilitate the doping of the X element into the SrTiO3 lattice during hydrothermal;
[0018] S2, preparation of X-SrTiO3 / TiO2 S-type heterojunction, X-SrTiO3 powder and tetrabutyl titanate in S1 are dissolved in ethanol and glycerol, ultrasonicated for 10 minutes, and stirred for 10 minutes, and then the mixed suspension is transferred to a high-pressure hydrothermal autoclave lined with polytetrafluoroethylene and placed in an oven for heating; after the hydrothermal autoclave is naturally cooled, the reaction precipitate is separated, repeatedly washed with ethanol, placed in a vacuum drying oven, and dried to obtain X-SrTiO3 / TiO2 powder; the mixed material is subjected to an operation of first ultrasonication and then stirring, the purpose of which is to first ultrasonically break large particles of X-SrTiO3 to form a homogeneous suspension, and then stir to make tetrabutyl titanate evenly adhere to the Fe-SrTiO3 powder, so as to facilitate the preparation of Fe-SrTiO3 / TiO2 with uniform particles.
[0019] Furthermore, in the above S1, the molar ratio of tetrabutyl titanate to ethanolamine is 1:(1.5-2.5).
[0020] Furthermore, in the above S1, the volume ratio of the added NaOH solution to the ethanolamine solution is 1:(1-1.5).
[0021] Furthermore, in the above S1, the mass fraction of the NaOH solution is 36-40%.
[0022] Furthermore, in the above S1, the concentration of strontium nitrate in the mixed aqueous solution of strontium nitrate and the nitrate of X is 1 to 1.2 mol / L.
[0023] Furthermore, in the above S1, the molar ratio of the nitrate concentration of X to the strontium nitrate concentration is 1:(10-200).
[0024] Furthermore, in the above S1, the ratio of the added volume of the mixed aqueous solution of strontium nitrate and the nitrate of X to the volume of the NaOH solution is 1:(5-6).
[0025] Furthermore, in the above S1, the temperature in the oven is set to 160-200°C, and the continuous heating time is 24-30 hours.
[0026] Furthermore, in the above S1, the temperature of the vacuum drying oven is 60-70°C, and the heating is continued for 12-24 hours.
[0027] Furthermore, in the above S2, the molar ratio of tetrabutyl titanate to X-SrTiO3 is 1:(1 to 1.5).
[0028] Furthermore, in the above S2, the mass ratio of ethanol to X-SrTiO3 is 1:(10-15).
[0029] Furthermore, in the above S2, the mass ratio of glycerol to ethanol is 1:(1.8-2).
[0030] Furthermore, in the above S2, the temperature in the oven is set to 160-180°C, and the continuous heating time is 24-30 hours.
[0031] Furthermore, in the above S2, the temperature of the vacuum drying oven is 60-70°C, and the heating is continued for 12-24 hours.
[0032] Furthermore, in the above preparation method, when X is Fe element, the nitrate of X is iron nitrate; when X is Cu element, the nitrate of X is copper nitrate; when X is Ce element, the nitrate of X is cerium nitrate; when X is Ag element, the nitrate of X is silver nitrate; when X is Pd element, the nitrate of X is palladium nitrate.
[0033] The present application also provides an application of the above-mentioned metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2 in the treatment of nitrogen-containing wastewater, including applying the photocatalytic material X-SrTiO3 / TiO2 to the photocatalytic reduction of nitrate process, wherein the strong reducing photogenerated electrons provided by SrTiO3 / TiO2 and the strong adsorption capacity provided by X jointly improve the denitrification performance of the material, thereby achieving the purpose of reducing the photocatalytic material and formic acid.
[0034] The present application also provides a photocatalytic denitrification process for treating nitrate-containing wastewater, comprising adding the above-mentioned S-type heterojunction photocatalytic material X-SrTiO3 / TiO2 and formic acid to the nitrate-containing wastewater, and performing a denitrification reaction by photocatalysis.
[0035] Furthermore, the nitrate in the above nitrate wastewater includes NaNO3, KNO3 and other NO3 - Salt, wherein the NO3-N concentration is 50 ~ 200 mg / L.
[0036] Furthermore, the dosage of the above-mentioned X-SrTiO3 / TiO2 is 0.1‰ to 0.5‰ of the mass of the nitrate wastewater solution.
[0037] Furthermore, the formic acid is used in an amount of 0 mmol / L to 60 mmol / L. Furthermore, the formic acid is used in an amount of 20 mmol / L to 60 mmol / L.
[0038] Furthermore, the above-mentioned photocatalysis is ultraviolet light, and the illumination power is 500-1000W.
[0039] Furthermore, the above-mentioned photocatalytic denitrification process is carried out in a photocatalytic reactor.
[0040] 3. Beneficial effects
[0041] Compared with the prior art, the present application has the following beneficial effects:
[0042] (1) The present application provides a metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2, wherein X is a metal element, including Fe, Cu, Ce, Ag or Pd, and X is doped into the SrTiO3 lattice to form a coupled heterostructure with anatase TiO2. SrTiO3 and TiO2 construct a built-in electric field so that the Fermi levels of the two are arranged in the same position, forming an S-type heterojunction. Under ultraviolet light irradiation, the low-oxidizing photogenerated holes in the SrTiO3 valence band recombine with the low-reducing photogenerated electrons in the TiO2 conduction band, so that the high-reducing photogenerated electrons in the SrTiO3 conduction band are preserved and enriched. Metal elements such as Fe, Cu or Ce are doped into the SrTiO3 lattice, and metal elements such as Fe are used as NO3 - The anchoring point can significantly enhance the material's resistance to NO3 - The adsorption capacity of NO3 is combined with the high reduction capacity of photogenerated electrons in the S-type heterojunction. - Direct reduction on the heterojunction becomes dominant. And the strong adsorption capacity can make NO3 - and intermediate NO2 - It is adsorbed on the surface of the material in large quantities, increasing NO3 - The ratio of electrons to avoid a large number of electrons reacting with one NO3 - The reaction converts it into NH4 + At this time, a small amount of formic acid is added to consume the photogenerated holes with high oxidation capacity in TiO2, avoiding the oxidation reaction intermediate NO2 - , and can produce a small amount of CO2 - Further improve nitrate conversion rate and N2 selectivity.
[0043] (2) The present application provides a metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2, which has strong reducing electrons and strong adsorption capacity, so that a small amount of photocatalytic material can achieve high denitrification performance. In the experiment, 100-400 mg / L of photocatalytic material was used, combined with 20-40 mmol / L of formic acid to reduce 100 mg / L NO3-N to achieve a conversion rate of more than 95% and a N2 selectivity of more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 is a TEM image of Fe-SrTiO3 / TiO2 in the present invention;
[0045] Figure 2 is a TEM image of Fe-SrTiO3 in the present invention;
[0046] Figure 3 is a TEM image of Cu-SrTiO3 / TiO2 in the present invention;
[0047] Figure 4 is the XRD diagram of Fe-SrTiO3 / TiO2 and Cu-SrTiO3 / TiO2 in the present invention;
[0048] Figure 5 It is the ESR diagram of Fe-SrTiO3 / TiO2 and Cu-SrTiO3 / TiO2 in the present invention;
[0049] Figure 6 This is the nitrate reduction effect of Fe-SrTiO3 / TiO2 recovery and recycling in Example 4 of the present invention. DETAILED DESCRIPTION
[0050] The present application is further described below in conjunction with specific embodiments.
[0051] It should be noted that the terms such as "upper", "lower", "left", "right", "middle", etc. cited in this specification are only for the convenience of description and are not used to limit the scope of implementation. Changes or adjustments to their relative relationships should be regarded as the scope of implementation of this application without substantially changing the technical content.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.
[0053] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased from the market.
[0054] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.
[0055] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.
[0056] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.
[0057] Example 1
[0058] This embodiment provides a metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2 and a preparation method thereof, wherein X is Fe element, and Fe element is doped into the SrTiO3 lattice to form a coupled heterostructure with anatase TiO2. The preparation method comprises the following steps:
[0059] S1, take 0.5g ethanolamine and add it to 20ml deionized water, stir at room temperature until it is fully dissolved, then slowly add 1.7g tetrabutyl titanate, continue stirring for 10min, add 25ml NaOH solution (36%) to the mixed solution, then add 5ml 1mol / L strontium nitrate and 0.02mol / L ferric nitrate mixed aqueous solution to form a yellow suspension, continue stirring for 30min, then transfer to a high-pressure hydrothermal autoclave lined with tetrafluoroethylene, and place it in an oven and heat it at 200℃ for 24h; after natural cooling, separate the light yellow precipitate of the reaction, wash it repeatedly with ethanol and deionized water, and dry it to obtain Fe-SrTiO3 powder;
[0060] S2, take 1.1g of the above Fe-SrTiO3 powder and 1.7g of tetrabutyl titanate and dissolve them in a mixed solution of 30ml of ethanol and 15ml of glycerol, ultrasonicate for 10min, and then stir for 10min, transfer the mixed suspension to a high-pressure hydrothermal autoclave lined with polytetrafluoroethylene, and heat it in an oven; after natural cooling, separate the reaction precipitate, wash it repeatedly with ethanol, and dry it to obtain Fe-SrTiO3 / TiO2 powder.
[0061] Result analysis:
[0062] The Fe-SrTiO3 / TiO2 powder and Fe-SrTiO3 powder obtained above were characterized by TEM. Figure 1 and Figure 2As shown, the material is a nanorod cluster structure, and the dispersion of Fe-SrTiO3 / TiO2 is better than that of Fe-SrTiO3; the Fe-SrTiO3 / TiO2 powder obtained above was characterized by XRD, and the results are as follows Figure 4 As shown, the characteristic peaks are consistent with the standard spectra of SrTiO3 and TiO2, the titanium dioxide crystal form is taceous, and no absorption peaks of Fe element or oxidation state are found, indicating that Fe has been completely doped into the SrTiO3 lattice.
[0063] The Fe-SrTiO3 / TiO2 powder obtained above was characterized by ESR. - The free radical experiment tests the reduction performance of the material, and the results are as follows Figure 5 As shown, TiO2 has no O2 - The generation of free radicals indicates that the conduction band potential of TiO2 is not negative enough. The peak intensity in Fe-SrTiO3 / TiO2 is significantly higher than that in Fe-SrTiO3, proving that Fe-SrTiO3 / TiO2 has stronger reducing properties and carrier separation effects.
[0064] Example 2
[0065] This embodiment provides a metal-doped SrTiO3 / TiO2 S-type heterojunction photocatalytic material X-SrTiO3 / TiO2 and a preparation method thereof, wherein X is a Cu element, and the Cu element is doped into the SrTiO3 lattice to form a coupled heterostructure with anatase TiO2. The preparation method comprises the following steps:
[0066] S1, take 0.5g ethanolamine and add it to 20ml deionized water, stir at room temperature until it is fully dissolved, then slowly add 1.7g tetrabutyl titanate, continue stirring for 10min, add 25ml NaOH solution (36%) to the mixed solution, then add 5ml 1mol / L strontium nitrate and 0.02mol / L copper nitrate mixed aqueous solution to form a blue suspension, continue stirring for 30min, then transfer to a high-pressure hydrothermal autoclave lined with tetrafluoroethylene, and place it in an oven and heat it at 200℃ for 24h; after natural cooling, separate the light blue precipitate of the reaction, wash it repeatedly with ethanol and deionized water, and dry it to obtain Cu-SrTiO3 powder;
[0067] S2, take 1.1g of the above-mentioned Cu-SrTiO3 powder and 1.7g of tetrabutyl titanate and dissolve them in a mixed solution of 30ml of ethanol and 15ml of glycerol, ultrasonicate for 10min, and then stir for 10min, transfer the mixed suspension to a high-pressure hydrothermal autoclave lined with polytetrafluoroethylene, and heat it in an oven; after natural cooling, separate the reaction precipitate, wash it repeatedly with ethanol, and dry it to obtain Cu-SrTiO3 / TiO2 powder.
[0068] Result analysis:
[0069] The Cu-SrTiO3 / TiO2 powder obtained above was characterized by TEM and XRD. Figure 3 and Figure 4 As shown, similar to Fe-SrTiO3 / TiO2, the Cu-SrTiO3 / TiO2 powder is a nanorod cluster structure, the titanium dioxide crystal form is taceous, and no absorption peaks of Cu single substance or oxidation state are found, indicating that Cu has been completely doped into the SrTiO3 lattice.
[0070] The Cu-SrTiO3 / TiO2 powder obtained above was characterized by ESR. - The free radical experiment tests the reduction performance of the material, and the results are as follows Figure 5 As shown, the peak intensity in Cu-SrTiO3 / TiO2 is second only to Fe-SrTiO3 / TiO2 in Example 1, proving that Cu-SrTiO3 / TiO2 also has strong reducing properties and carrier separation effects.
[0071] Example 3
[0072] This example provides the application of Fe-SrTiO3 / TiO2 prepared in Example 1 in the photocatalytic reduction of nitrate.
[0073] Prepare 7.15mol / L NaNO3 aqueous solution, take out 1000ml, and prepare 100mgN / L simulated solution. Take 250mg Fe-SrTiO3 / TiO2 powder prepared in Example 1, add simulated solution after adsorption saturation, then add 20mmol formic acid (98%) to the simulated solution, react for 60min under medium pressure ultraviolet lamp (1000W), take samples at 0min and every 10min thereafter, and measure the nitrate nitrogen, nitrite nitrogen and ammonia nitrogen content in the samples. The changes in nitrate nitrogen, nitrite nitrogen and ammonia nitrogen concentration (mg / L) are shown in Table 1.
[0074] Table 1
[0075]
[0076] Example 4
[0077] This embodiment provides the use of recovered Fe-SrTiO3 / TiO2 in photocatalytic reduction of nitrates.
[0078] Referring to Example 3, the Fe-SrTiO3 / TiO2 after the reaction was filtered, and dried in a vacuum drying oven at 60°C for more than 12 hours, and the above photocatalytic experiment was repeated. The nitrate removal effect and nitrogen selectivity of the Fe-SrTiO3 / TiO2 after repeated use for 5 times were as follows: Figure 4 shown.
[0079] Example 5
[0080] This example provides the application of Cu-SrTiO3 / TiO2 prepared in Example 2 in the photocatalytic reduction of nitrate.
[0081] Prepare 7.15mol / L NaNO3 aqueous solution, take out 1000ml, and obtain 100mg N / L simulated solution. Take 250mg Cu-SrTiO3 / TiO2 powder prepared in Example 2, add simulated solution after adsorption saturation, then add 20mmol formic acid (98%) to the simulated solution, react for 60min under medium pressure ultraviolet lamp (1000W), take samples at 0min and every 10min thereafter, and measure the nitrate nitrogen, nitrite nitrogen and ammonia nitrogen content in the samples. The changes in nitrate nitrogen, nitrite nitrogen and ammonia nitrogen concentration (mg / L) are shown in Table 2.
[0082] Table 2
[0083]
[0084] Example 6
[0085] This embodiment provides a photocatalytic reduction process of nitrate with different formic acid dosages.
[0086] Refer to Example 3, the difference is that the dosage of formic acid in the photocatalytic reduction of nitrate is 0mmol / L, 20mmol / L, 40mmol / L, and 60mmol / L, respectively, the photocatalytic reaction is 60min, and the nitrate conversion rate and nitrogen selectivity are measured respectively, as shown in the following table.
[0087] Table 3
[0088] Formic acid dosage mmol / L <![CDATA[NO3- conversion rate %]]> <![CDATA[% N2 Selectivity]]> 0 53.64 35.11 20 95.72 96.26 40 97.39 97.12 60 97.55 95.69
[0089] Comparative Example
[0090] This comparative example provides a metal-free SrTiO3 / TiO2 S-type heterojunction photocatalytic material SrTiO3 / TiO2 and a preparation method thereof. The preparation method is similar to that of Example 1, except that only 5 ml of 1 mol / L strontium nitrate aqueous solution is added dropwise in step S1, specifically comprising:
[0091] S1, take 0.5g ethanolamine and add it into 20ml deionized water, stir at room temperature until it is fully dissolved, then slowly drop 1.7g tetrabutyl titanate, continue stirring for 10min, drop 25ml NaOH solution (36%) into the mixed solution, then drop 5ml 1mol / L strontium nitrate aqueous solution, continue stirring for 30min, transfer to a high-pressure hydrothermal autoclave lined with tetrafluoroethylene, and place in an oven and heat at 200℃ for 24h; separate the reaction precipitate after natural cooling, wash repeatedly with ethanol and deionized water, and dry to obtain SrTiO3 powder;
[0092] S2, take 1.1g of the above SrTiO3 powder and 1.7g of tetrabutyl titanate and dissolve them in a mixed solution of 30ml of ethanol and 15ml of glycerol, ultrasonicate for 10min, and then stir for 10min, transfer the mixed suspension to a high-pressure hydrothermal autoclave lined with polytetrafluoroethylene, and heat it in an oven; after natural cooling, separate the reaction precipitate, wash it repeatedly with ethanol, and dry it to obtain SrTiO3 / TiO2 powder.
[0093] Prepare 7.15mol / L NaNO3 aqueous solution, take out 1000ml, and prepare 100mgN / L simulated solution. Take 250mg of the above SrTiO3 / TiO2 powder, add simulated solution after adsorption saturation, then add 20mmol formic acid (98%) to the simulated solution, react for 60min under medium pressure ultraviolet lamp (1000W), take samples at 0min and every 10min thereafter, and determine the content of nitrate nitrogen, nitrite nitrogen and ammonia nitrogen in the samples. The changes in nitrate nitrogen, nitrite nitrogen and ammonia nitrogen concentration (mg / L) are shown in Table 4.
[0094] Table 4
[0095]
Claims
1. A photocatalytic degradation process for treating nitrate-containing wastewater, characterized in that: The process comprises adding an S-type heterojunction photocatalytic material X-SrTiO3 / TiO2 and formic acid to nitrate-containing wastewater, and performing a denitrification reaction by photocatalysis, wherein X is a metal element that makes the surface of the material Lewis acid after doping, and X-SrTiO3 / TiO2 is a coupled heterostructure formed by X doped into the SrTiO3 lattice and anatase-type TiO2; The metal element includes Fe, Cu, Ce, Ag or Pd.
2. The process according to claim 1, characterized in that The dosage of X-SrTiO3 / TiO2 is 0.1‰~0.5‰ of the mass of the nitrate wastewater solution; the usage of formic acid is 20 mmol / L~60 mmol / L.
3. The process according to claim 2, characterized in that In the X-SrTiO3 / TiO2, the molar ratio of TiO2 to Sr element is 1:1-1.5; and / or the molar ratio of metal element to Sr element is 1:10-200.
4. The process according to any one of claims 1 to 3, characterized in that: The preparation method of the S-type heterojunction photocatalytic material X-SrTiO3 / TiO2 comprises the following steps: S1, preparation of X-doped SrTiO3, under stirring at room temperature, slowly drop tetrabutyl titanate into an ethanolamine aqueous solution, after stirring, drop NaOH solution into the mixed solution, drop strontium nitrate and a mixed aqueous solution of X nitrate, ultrasonicate, continue stirring, transfer to a high-pressure hydrothermal autoclave, and heat; after cooling the hydrothermal autoclave, separate the reaction precipitate, repeatedly wash with ethanol and deionized water, and dry to obtain X-SrTiO3 powder; S2, preparation of X-SrTiO3 / TiO2 S-type heterojunction, dissolving the X-SrTiO3 powder and tetrabutyl titanate in S1 in ethanol and glycerol, ultrasonicating, stirring, and then transferring the mixed suspension to a high-pressure hydrothermal autoclave and heating; after the hydrothermal autoclave is cooled, the reaction precipitate is separated, washed with ethanol, and dried to obtain X-SrTiO3 / TiO2 powder.
5. The process according to claim 4, characterized in that In S1, The molar ratio of tetrabutyl titanate to ethanolamine is 1:1.5-2.5; and / or the ratio of the added volume of the NaOH solution to the volume of the ethanolamine solution is 1:1 to 1.5; and / or a mixed aqueous solution of strontium nitrate and the nitrate of X, wherein the concentration of strontium nitrate is 1 to 1.2 mol / L; and / or the molar ratio of the nitrate concentration of X to the strontium nitrate concentration is 1:10 to 200; The ratio of the added volume of the mixed aqueous solution of strontium nitrate and / or X nitrate to the volume of the NaOH solution is 1:5-6.
6. The process according to claim 5, characterized in that In S2, The molar ratio of tetrabutyl titanate to X-SrTiO3 is 1:1~1.5; and / or the mass ratio of ethanol to X-SrTiO3 is 1:10~15; And / or the mass ratio of glycerol to ethanol is 1:1.8~2.
7. The process according to claim 6, characterized in that When X is Fe, the nitrate of X is iron nitrate; when X is Cu, the nitrate of X is copper nitrate; when X is Ce, the nitrate of X is cerium nitrate; when X is Ag, the nitrate of X is silver nitrate; when X is Pd, the nitrate of X is palladium nitrate.
Citation Information
Cited By
Preparation method for in-situ etching growth nested SrTiO3 / TiO2 heterojunction photocatalytic material