Polyethylene / functional polystyrene nano-microsphere composite insulating resin and its preparation method and application

By combining functionalized polystyrene nanomicrospheres with polyethylene resin, the problem of poor dispersion of inorganic nanoparticles is solved, and the electrical resistance and insulation performance of polyethylene resin are significantly improved, thereby realizing the preparation of high-performance insulating materials.

CN117624799BActive Publication Date: 2024-11-08NANTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311729567.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-11-08
Estimated Expiration
2043-12-15

AI Technical Summary

Technical Problem

The dispersion of inorganic nanoparticles in polyethylene resins is poor, resulting in limited electrical insulation performance of insulating materials and difficult to improve electrical resistance.

Method used

Functional polystyrene nanomicrospheres are used to coat polystyrene cross-link nanomicrospheres by polypyrrole to form a uniformly dispersed polyethylene/functional polystyrene nanomicrosphere composite insulating resin, and prepared by emulsion polymerization method and combined with polyethylene. Resin refining to form high-performance insulating materials.

Benefits of technology

The electrical resistance strength of polyethylene resin has been significantly improved, the DC breakdown strength reaches 380-460kV/mm, and the volume resistivity is increased by 1.5-4 times, solving the problem of poor dispersion of inorganic nanoparticles and improving the insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004609731000000051
    Figure BDA0004609731000000051
Patent Text Reader

Abstract

The present invention relates to the technical field of insulating resins, and in particular to a polyethylene / functional polystyrene nanosphere composite insulating resin and a preparation method and application thereof. The polyethylene / functional polystyrene nanosphere composite insulating resin of the present invention is composed of 99-99.99wt% of polyethylene resin and 0.01-1wt% of functional polystyrene nanospheres. In the polyethylene / functional polystyrene nanosphere composite insulating resin of the present invention, traditional inorganic nanometers are replaced by organic polystyrene nanospheres, which solves the problem of uneven dispersion of inorganic nanometers in polymers; at the same time, the polystyrene nanospheres are functionalized, which effectively improves the electrical breakdown strength and volume resistivity of the composite material, the DC breakdown strength is maintained between 380-460kV / mm, and the volume resistivity is increased by 1.5-4 times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of insulating resins, and in particular to a polyethylene / functional polystyrene nano-microsphere composite insulating resin and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy, urban electricity load is increasing sharply. The development of new energy power generation, long-distance transmission and smart grid has led to the rapid development of high-voltage direct current transmission technology. As the key equipment of high-voltage direct current transmission, the transmission voltage level of high-voltage direct current transmission cable determines the technical level of high-voltage direct current transmission. Among them, improving the electrical strength of insulating materials is the core of improving the transmission voltage level of high-voltage direct current transmission cables. Improving the electrical strength of insulating materials can reduce the size of DC cables at the same level, which has the effect of reducing cable weight and production costs; under the same cable size, it can greatly increase the transmission voltage, increase the power transmission rate, and reduce power loss.

[0003] In order to improve the electrical strength of insulating materials, scientists and engineers have developed many technologies, among which blending modification, inorganic nanofilling and grafting modification are the most important technical solutions. Compared with grafting modification and blending modification, inorganic nanofilling technology has received greater attention. Available nanoparticles include nano-silicon dioxide, nano-metal oxides, inorganic non-metallic nanoparticles, including nano-silicon carbide, boron nitride, etc. The addition of nanomaterials can not only improve the electrical strength of insulating materials, but also inhibit the growth of electrical trees, resist corona aging, and reduce space charge accumulation.

[0004] However, inorganic nanoparticles have high surface energy, are very easy to agglomerate, and are difficult to disperse in resins. Therefore, the dispersibility of inorganic nanoparticles is the biggest obstacle to the development of nano-electrical insulating composite materials. Although the dispersibility of inorganic nanoparticles can be partially improved by surface modification, it is impossible to make inorganic nanoparticles interact strongly with polyethylene resin, which limits the electrical insulation performance of nano-modified insulating materials. Summary of the invention

[0005] In view of the above problems, the present invention provides a polyethylene / functional polystyrene nanosphere composite insulating resin and a preparation method and application thereof, in which organic nanomaterials are used to replace inorganic nanomaterials. The functional polystyrene nanospheres have the characteristics of uniform particle size and monodispersity, and can be evenly dispersed in the polyethylene resin, thus solving the problem of the difficulty in dispersing inorganic nanoparticles in the polyethylene resin and improving the electrical strength of the polyethylene.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A polyethylene / functional polystyrene nano-microsphere composite insulating resin, which is composed of 99-99.99wt% polyethylene resin and 0.01-1wt% functional polystyrene nano-microspheres;

[0008] The functional polystyrene nano-microspheres are cross-linked polystyrene nano-microspheres coated with polypyrrole;

[0009] The cross-linked polystyrene nanospheres are prepared from styrene monomer and cross-linking agent divinylbenzene by emulsion polymerization;

[0010] The polypyrrole is obtained by polymerizing one of pyrrole and 3-methylpyrrole or a mixture of the two in any mass ratio.

[0011] Preferably, the polyethylene resin is a low-density polyethylene resin or a linear low-density polyethylene resin, and the linear low-density polyethylene resin is one or more of ethylene-1-butene copolymer, ethylene-1-hexene copolymer and ethylene-1-octene copolymer.

[0012] Preferably, the diameter of the functional polystyrene nanospheres is 50-300 nanometers.

[0013] Preferably, in the polystyrene cross-linked nano-microspheres, the content of the cross-linking agent divinylbenzene is 2-4wt%.

[0014] The present invention also provides a method for preparing a polyethylene / functional polystyrene nano-microsphere composite insulating resin, comprising the following steps:

[0015] Step 1: Preparation of polystyrene cross-linked nanospheres

[0016] The styrene monomer and the cross-linking agent divinylbenzene are prepared into a monomer mixture in a mass ratio of 96-98:2-4, and the prepared monomer mixture, deionized water and emulsifier sodium dodecyl sulfate are added into a three-necked flask in a weight ratio of 8:100:0.05-0.15, stirred, and nitrogen is passed through, the temperature is raised to 75°C, an initiator is added, the reaction is performed for 8 hours, and the reaction is stopped; the amount of the initiator is 3wt% of the total mass of the monomer; after the reaction is completed, centrifuge at 10000rpm, remove the supernatant, add deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again; repeat 3 times to remove unreacted monomers and other small molecular impurities; the washed polystyrene cross-linked nanospheres are re-dispersed in deionized water to prepare a dispersion with a concentration of 5wt% for standby use;

[0017] Step 2: Preparation of functional polystyrene nanospheres

[0018] The polystyrene cross-linked nanosphere dispersion prepared in step 1 is dispersed in deionized water to prepare a 1wt% dispersion, and ammonium persulfate is dissolved in deionized water to prepare a 5wt% aqueous solution; pyrrole monomer and ammonium persulfate aqueous solution are added to the dispersion under stirring conditions, and the reaction is continued for 48 hours; wherein the molar ratio of pyrrole monomer to ammonium persulfate is 4:1; centrifugation is performed at 10000rpm using a centrifuge, the supernatant is removed, anhydrous ethanol is added, ultrasonic dispersion is performed for 30 minutes, and then centrifugation is repeated 3 times to remove unreacted monomers and other small molecular impurities; the washed product is placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres;

[0019] Step 3: Preparation of polyethylene / functional polystyrene nanosphere composite insulating resin

[0020] The polyethylene resin and the functional polystyrene nano-microspheres prepared in step 2 are weighed according to the ratio, and the components are added into an internal mixer for internal mixing to obtain a polyethylene / functional polystyrene nano-microsphere composite insulating resin.

[0021] Preferably, in step 1, the initiator is potassium persulfate.

[0022] Preferably, in step 2, the pyrrole monomer is pyrrole, 3-methylpyrrole or a mixture of the two in any mass ratio.

[0023] Preferably, in step 2, the weight ratio of the pyrrole monomer to the polystyrene nanospheres is 1:8-14.

[0024] Preferably, in step three, the banburying temperature is 180-190° C., the banburying time is 6-10 min, and the banburying speed is 60 rpm.

[0025] The present invention also provides an application of the polyethylene / functional polystyrene nano-microsphere composite insulating resin prepared by the above preparation method as an insulating material for high-voltage direct current transmission cables, specifically:

[0026] The polyethylene / functional polystyrene nanosphere composite insulating resin of the present invention can be directly used as an insulating material for high-voltage DC power cables, or can be mixed with a crosslinking agent, a voltage stabilizer, functional grafted polyethylene, etc. in the form of a masterbatch to prepare a crosslinked polyethylene cable.

[0027] Beneficial effects of the present invention:

[0028] 1. The present invention replaces inorganic nanoparticles with organic nanoparticles. Compared with inorganic nanoparticles, organic nanoparticles have lower surface energy, are not easy to agglomerate after polymerization, and are in a monodisperse state. They have good wettability with polyethylene resin and can be evenly dispersed in the polymer, which is conducive to industrial-scale application.

[0029] 2. In the functional nano-microspheres formed by coating the polystyrene nano-microspheres with polypyrrole, the highly conjugated macromolecular structure of polypyrrole helps to dissipate the energy of injected high-energy electrons, thereby avoiding the damage of high-energy electrons to the polyethylene molecular chains, and can significantly improve the electrical strength of the polyethylene resin. The DC breakdown test shows that the DC breakdown strength of the polyethylene / functional polystyrene nano-microsphere composite insulating resin of the present invention reaches 380-460 kV / mm, which is much higher than the breakdown strength of the polyethylene resin of 285-296 kV / mm. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is further illustrated and described below through specific implementation modes, but the implementation modes of the present invention are not limited thereto.

[0031] A polyethylene / functional polystyrene nano-microsphere composite insulating resin is composed of 99-99.99wt% of polyethylene resin and 0.01-1wt% of functional polystyrene nano-microsphere.

[0032] Wherein, the functional polystyrene nano-microspheres are polypyrrole-coated polystyrene cross-linked nano-microspheres;

[0033] The cross-linked polystyrene nanospheres are prepared from styrene monomer and cross-linking agent divinylbenzene by emulsion polymerization;

[0034] The polypyrrole is obtained by polymerizing one of pyrrole and 3-methylpyrrole or a mixture of the two in any mass ratio.

[0035] A method for preparing a polyethylene / functional polystyrene nano-microsphere composite insulating resin comprises the following steps:

[0036] Step 1: Preparation of polystyrene cross-linked nanospheres

[0037] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture according to a mass ratio of (96-98): (2-4), and the configured monomer mixture, deionized water and emulsifier sodium dodecyl sulfate are added into a three-necked flask according to a weight ratio of 8:100: (0.05-0.15) and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, an initiator is added, and the reaction is performed for 8 hours, and the reaction is stopped. The amount of the initiator is 3wt% of the total mass of the monomer. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to form a dispersion with a concentration of 5wt% for standby use.

[0038] Wherein, the initiator is potassium persulfate, and the content of the cross-linking agent divinylbenzene is 2-4wt%.

[0039] Step 2: Preparation of functional polystyrene nanospheres

[0040] The polystyrene cross-linked nanosphere dispersion prepared in step 1 is dispersed in deionized water to prepare a 1wt% dispersion. Ammonium persulfate is dissolved in deionized water to prepare a 5wt% aqueous solution. Pyrrole monomer and ammonium persulfate aqueous solution are added to the dispersion under stirring conditions, and the reaction is continued for 48 hours. The weight ratio of pyrrole monomer to polystyrene microspheres is 1:(8-14), and the molar ratio of pyrrole monomer to ammonium persulfate is 4:1. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, add anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecule impurities.

[0041] The washed product was dried in a vacuum drying oven at 50° C. to obtain functional polystyrene nanospheres.

[0042] The pyrrole monomer is one of pyrrole and 3-methylpyrrole or a mixture of the two in any mass ratio. The diameter of the prepared functional polystyrene nanospheres is 50-300 nanometers.

[0043] Step 3: Preparation of polyethylene / functional polystyrene nanosphere composite insulating resin

[0044] Weigh polyethylene resin and functional polystyrene nanospheres prepared in step 2 according to the ratio, add the components into an internal mixer for internal mixing at a temperature of 180-190° C., a mixing time of 6-10 min, and a mixing speed of 60 rpm to obtain polyethylene / functional polystyrene nanosphere composite insulating resin.

[0045] The polyethylene resin is a low-density polyethylene resin or a linear low-density polyethylene resin, and the linear low-density polyethylene resin is one or more of ethylene-1-butene copolymer, ethylene-1-hexene copolymer, and ethylene-1-octene copolymer.

[0046] The present invention also provides an application of the polyethylene / functional polystyrene nano-microsphere composite insulating resin prepared by the above preparation method as an insulating material for high-voltage direct current transmission cables, specifically:

[0047] The polyethylene / functional polystyrene nanosphere composite insulating resin of the present invention can be directly used as an insulating material for high-voltage DC power cables, or can be mixed with a crosslinking agent, a voltage stabilizer, functional grafted polyethylene, etc. in the form of a masterbatch to prepare a crosslinked polyethylene cable.

[0048] The DC breakdown test is conducted in accordance with GB / T1408.1-2016 and GB / T1408.2-2016 standards. A linearly increasing DC voltage is applied to the insulating material (75μm thick film sample) at a voltage increase rate of 1kV / mm until the sample breaks down. Each sample is tested 10 times and the average breakdown strength is calculated.

[0049] Volume resistivity measurement method: At 70°C, apply a 30kV / mm DC electric field to the insulating material, use an electrometer to collect the leakage current, and calculate the volume resistivity based on the test current. The formula is as follows:

[0050]

[0051] Wherein, ρ is the volume resistivity, unit: Ω·m; I is the measured leakage current, unit: A; E is the electric field strength, 30 kV / mm; S is the test electrode area, and the electrode diameter is 50 mm.

[0052] Example 1

[0053] Step 1

[0054] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture according to a mass ratio of 98:2. 160g of the monomer mixture, 2000mL of deionized water and 1g of sodium dodecylsulfonate are added to a 5L three-necked flask and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, and 4.8g of initiator potassium persulfate is added. The reaction is stopped for 8 hours. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to form a dispersion with a concentration of 5wt% for standby use.

[0055] Step 2

[0056] Disperse 1000mL of the prepared polystyrene cross-linked nanosphere dispersion in 4000mL of deionized water to prepare a 1wt% dispersion. Dissolve ammonium persulfate in deionized water to prepare a 5wt% aqueous solution. Add 5g of pyrrole and 85mL of ammonium persulfate aqueous solution to the dispersion under stirring conditions, and the reaction lasts for 48 hours. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, put into anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. Obtain polystyrene cross-linked nanospheres with an average particle size of 300 nanometers. The washed product is placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres.

[0057] Step 3

[0058] Weigh 99.5 parts by weight of linear low-density polyethylene resin and 0.5 parts by weight of the functional polystyrene nanospheres prepared in step 2, add the components to an internal mixer and mix them at a temperature of 190° C., a mixing time of 6 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0059] DC breakdown strength: 423kV / mm, volume resistivity: 6.5ⅹ10 14 Ω·m.

[0060] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0061] Example 2

[0062] Step 1 and step 2 are the same as those in Example 1, except that:

[0063] Step 3

[0064] Weigh 99.9 parts by weight of linear low-density polyethylene resin and 0.1 parts by weight of the functional polystyrene nanospheres prepared in step 2, add the components to an internal mixer and mix them at a mixing temperature of 190° C., a mixing time of 6 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0065] DC breakdown strength: 387kV / mm, volume resistivity: 1.1ⅹ10 15 Ω·m.

[0066] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0067] Example 3

[0068] Step 1 and step 2 are the same as those in Example 1, except that:

[0069] Step 3

[0070] Weigh 99.99 parts by weight of linear low-density polyethylene resin and 0.01 parts by weight of the functional polystyrene nanospheres prepared in step 2, add the components to an internal mixer and mix them at a mixing temperature of 190° C., a mixing time of 6 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0071] DC breakdown strength: 382kV / mm, volume resistivity: 7.3ⅹ10 14 Ω·m.

[0072] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0073] Example 4

[0074] Step 1 and step 2 are the same as those in Example 1, except that:

[0075] Step 3

[0076] Weigh 99 parts by weight of linear low-density polyethylene resin and 1 part by weight of the functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer and mix them at a temperature of 190° C., a mixing time of 6 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0077] DC breakdown strength: 410kV / mm, volume resistivity: 5.3ⅹ10 14 Ω·m.

[0078] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0079] Example 5

[0080] Step 1

[0081] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture according to a mass ratio of 96:4. 160g of the monomer mixture, 2000mL of deionized water and 1.6g of sodium dodecylsulfonate are added to a 5L three-necked flask and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, and 4.8g of initiator potassium persulfate is added. The reaction is stopped for 8 hours. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to be configured into a dispersion with a concentration of 5wt% for standby use.

[0082] Step 2

[0083] 1000mL of the prepared polystyrene cross-linked nanosphere dispersion was dispersed in 4000mL of deionized water to prepare a 1wt% dispersion. Ammonium persulfate was dissolved in deionized water to prepare a 5wt% aqueous solution. 6.25g of pyrrole and 106mL of ammonium persulfate aqueous solution were added to the dispersion under stirring conditions, and the reaction lasted for 48 hours. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, put into anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. Polystyrene cross-linked nanospheres with an average particle size of 190 nanometers were obtained. The washed product was placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres.

[0084] Step 3

[0085] Weigh 99.5 parts by weight of linear low-density polyethylene resin and 0.5 parts by weight of functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer for internal mixing at a temperature of 190° C., a mixing time of 8 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0086] DC breakdown strength: 441kV / mm, volume resistivity: Volume resistivity: 5.8ⅹ10 14 Ω·m.

[0087] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0088] Example 6

[0089] Step 1 and step 2 are the same as those in Example 5, except that:

[0090] Step 3

[0091] Weigh 99.5 parts by weight of low-density polyethylene resin and 0.5 parts by weight of functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer for internal mixing at a temperature of 190° C., a mixing time of 8 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0092] DC breakdown strength: 394kV / mm, volume resistivity: Volume resistivity: 1.3ⅹ10 14 Ω·m.

[0093] The DC breakdown strength of low-density polyethylene resin was 285 kV / mm and the volume resistivity was 8.7 x 10 13 Ω·m.

[0094] Example 7

[0095] Step 1

[0096] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture according to a mass ratio of 97:3. 160g of the monomer mixture, 2000mL of deionized water and 2g of sodium dodecylsulfonate are added to a 5L three-necked flask and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, and 4.8g of initiator potassium persulfate is added. The reaction is stopped for 8 hours. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to be configured into a dispersion with a concentration of 5wt% for standby use.

[0097] Step 2

[0098] 1000mL of the prepared polystyrene cross-linked nanosphere dispersion was dispersed in 4000mL of deionized water to prepare a 1wt% dispersion. Ammonium persulfate was dissolved in deionized water to prepare a 5wt% aqueous solution. 3.57g of 3-methylpyrrole and 50mL of ammonium persulfate aqueous solution were added to the dispersion under stirring conditions, and the reaction lasted for 48 hours. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, put into anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. Polystyrene cross-linked nanospheres with an average particle size of 120 nanometers were obtained. The washed product was placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres.

[0099] Step 3

[0100] Weigh 99.5 parts by weight of linear low-density polyethylene resin and 0.5 parts by weight of functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer for internal mixing at a temperature of 190° C., a mixing time of 8 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0101] DC breakdown strength: 452kV / mm, volume resistivity: Volume resistivity: 8.5ⅹ10 14 Ω·m.

[0102] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0103] Example 8

[0104] Step 1

[0105] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture in a mass ratio of 97:3. 160g of the monomer mixture, 2000mL of deionized water and 3g of sodium dodecylsulfonate are added to a 5L three-necked flask and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, and 4.8g of initiator potassium persulfate is added. The reaction is stopped for 8 hours. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to be configured into a dispersion with a concentration of 5wt% for standby use.

[0106] Step 2

[0107] 1000mL of the prepared polystyrene cross-linked nanosphere dispersion was dispersed in 4000mL of deionized water to prepare a 1wt% dispersion. Ammonium persulfate was dissolved in deionized water to prepare a 5wt% aqueous solution. 2.5g of pyrrole and 2.5g of 3-methylpyrrole, and 77.5mL of ammonium persulfate aqueous solution were added to the dispersion under stirring conditions, and the reaction lasted for 48 hours. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, put into anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. Polystyrene cross-linked nanospheres with an average particle size of 50 nanometers were obtained. The washed product was placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres.

[0108] Step 3

[0109] Weigh 99.5 parts by weight of linear low-density polyethylene resin and 0.5 parts by weight of functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer and mix them at a temperature of 180° C., a mixing time of 10 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0110] DC breakdown strength: 458kV / mm, volume resistivity: Volume resistivity: 1.4ⅹ10 15 Ω·m.

[0111] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0112] Comparative Example 1: Styrene microspheres without surface coating

[0113] The other parts are the same as those in Example 1, except that the cross-linked polystyrene nanospheres are directly blended with the low-density polyethylene resin without further functionalization.

[0114] DC breakdown strength: 341kV / mm, volume resistivity: 4.3ⅹ10 14 Ω·m.

[0115] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0116] Comparative Example 2: Polypyrrole on the surface of styrene microspheres 1:5

[0117] Step 1

[0118] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture according to a mass ratio of 98:2. 160g of the monomer mixture, 2000mL of deionized water and 1g of sodium dodecylsulfonate are added to a 5L three-necked flask and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, and 4.8g of initiator potassium persulfate is added. The reaction is stopped for 8 hours. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to form a dispersion with a concentration of 5wt% for standby use.

[0119] Step 2

[0120] Disperse 1000mL of the prepared polystyrene cross-linked nanosphere dispersion in 4000mL of deionized water to prepare a 1wt% dispersion. Dissolve ammonium persulfate in deionized water to prepare a 5wt% aqueous solution. Add 10g of pyrrole and 170mL of ammonium persulfate aqueous solution to the dispersion under stirring conditions, and the reaction lasts for 48 hours. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, put into anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. Obtain polystyrene cross-linked nanospheres with an average particle size of 300 nanometers. The washed product is placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres.

[0121] Weigh 99.5 parts by weight of linear low-density polyethylene resin and 0.5 parts by weight of functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer for internal mixing at a temperature of 190° C., a mixing time of 6 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0122] DC breakdown strength: 353kV / mm, volume resistivity: 3.0ⅹ10 14 Ω·m.

[0123] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0124] Comparative Example 3: Polypyrrole on the surface of styrene microspheres 1:20

[0125] Step 1

[0126] The styrene monomer and the crosslinking agent divinylbenzene are configured into a monomer mixture according to a mass ratio of 98:2. 160g of the monomer mixture, 2000mL of deionized water and 1g of sodium dodecylsulfonate are added to a 5L three-necked flask and stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, and 4.8g of initiator potassium persulfate is added. The reaction is stopped for 8 hours. After the reaction is completed, centrifuge at 10000rpm, remove the supernatant, put into deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. The washed polystyrene crosslinked nanospheres are redispersed in deionized water to form a dispersion with a concentration of 5wt% for standby use.

[0127] Step 2

[0128] Disperse 1000mL of the prepared polystyrene cross-linked nanosphere dispersion in 4000mL of deionized water to prepare a 1wt% dispersion. Dissolve ammonium persulfate in deionized water to prepare a 5wt% aqueous solution. Add 2.5g of pyrrole and 42.5mL of ammonium persulfate aqueous solution to the dispersion under stirring conditions, and the reaction lasts for 48 hours. Centrifuge at 10000rpm using a centrifuge, remove the supernatant, put into anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again. Repeat 3 times to remove unreacted monomers and other small molecular impurities. Obtain polystyrene cross-linked nanospheres with an average particle size of 300 nanometers. The washed product is placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres.

[0129] Step 3

[0130] Weigh 99.5 parts by weight of linear low-density polyethylene resin and 0.5 parts by weight of functional polystyrene nanospheres prepared in step 2, add the components into an internal mixer for internal mixing at a temperature of 190° C., a mixing time of 6 min, and a mixing speed of 60 rpm to obtain a polyethylene / functional polystyrene nanosphere composite insulating resin.

[0131] DC breakdown strength: 353kV / mm, volume resistivity: 4.7ⅹ10 14 Ω·m.

[0132] The linear low-density polyethylene resin was tested, and the DC breakdown strength was 296 kV / mm and the volume resistivity was 3.4 x 10 14 Ω·m.

[0133] Comparing Example 1 with Comparative Example 1, the cross-linked polystyrene nanospheres were not functionalized, and the DC breakdown strength was reduced from 423 kV / mm to 341 kV / mm, and the volume resistivity was reduced from 6.5 x 10 14 Ω·m decreased to 4.7ⅹ10 14 Ω·m. This indicates that the functionalization of polystyrene cross-linked nanospheres with polypyrrole has a significant effect on improving the DC insulation properties of the resin.

[0134] Comparing Example 1 and Comparative Example 2, when the mass ratio of pyrrole monomer to polystyrene cross-linked nano-microspheres is too high during the functionalization process, the DC breakdown strength is reduced to 353 kV / mm, and the volume resistivity is reduced to a level lower than that of pure linear low-density polyethylene resin. Due to the increased conductivity of the thicker polypyrrole layer, the overall conductivity of the composite system is increased, and the breakdown strength is also reduced.

[0135] Comparing Example 1 and Comparative Example 3, when the mass ratio of pyrrole monomer to polystyrene cross-linked nano-microspheres is too low during the functionalization process, the improvement of DC breakdown strength and volume resistivity is also limited, indicating that a too thin polypyrrole layer does not significantly help improve the DC insulation performance of polyethylene.

[0136] Therefore, the polypyrrole functional layer on the surface of the functionalized polystyrene nanospheres should have an appropriate thickness in order to effectively improve the electrical breakdown strength of the insulating material.

[0137] In summary, in the polyethylene / functional polystyrene nanosphere composite insulating resin of the present invention, traditional inorganic nanoparticles are replaced by organic polystyrene nanospheres, thereby solving the problem of uneven dispersion of inorganic nanoparticles in the polymer; at the same time, the polystyrene nanospheres are functionalized, thereby effectively improving the electrical breakdown strength and volume resistivity of the composite material, the DC breakdown strength is maintained between 380 and 460 kV / mm, and the volume resistivity is increased by 1.5 to 4 times.

[0138] It should be noted that matters not described in detail in the present invention are all well-known technologies to those skilled in the art.

[0139] The above embodiments are only used to further illustrate the specific implementation methods of the present invention, but the present invention is not limited to the above embodiments. All equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are included in the protection scope of the technical solution of the present invention.

Claims

1. A polyethylene / functional polystyrene nanosphere composite insulating resin, characterized in that: It is composed of 99-99.99 wt% of polyethylene resin and 0.01-1 wt% of functional polystyrene nanospheres; The functional polystyrene nano-microspheres are cross-linked polystyrene nano-microspheres coated with polypyrrole; The polystyrene cross-linked nano-microspheres are prepared from styrene monomer and cross-linking agent divinylbenzene by emulsion polymerization; The polypyrrole is polymerized from one monomer of pyrrole and 3-methylpyrrole or a mixture of the two monomers in any mass ratio, and the weight ratio of the monomer to the polystyrene nanospheres is 1:8-14.

2. The polyethylene / functional polystyrene nanosphere composite insulating resin according to claim 1, characterized in that: The polyethylene resin is a low-density polyethylene resin or a linear low-density polyethylene resin, and the linear low-density polyethylene resin is one or more of ethylene-1-butene copolymer, ethylene-1-hexene copolymer, and ethylene-1-octene copolymer.

3. The polyethylene / functional polystyrene nano-microsphere composite insulating resin according to claim 1, characterized in that: The diameter of the functional polystyrene nanospheres is 50-300 nanometers.

4. The polyethylene / functional polystyrene nanosphere composite insulating resin according to claim 1, characterized in that: In the polystyrene cross-linked nano-microspheres, the content of the cross-linking agent divinylbenzene is 2-4 wt %.

5. The method for preparing a polyethylene / functional polystyrene nano-microsphere composite insulating resin according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Preparation of polystyrene cross-linked nanospheres The styrene monomer and the cross-linking agent divinylbenzene are prepared into a monomer mixture in a mass ratio of 96-98:2-4, and the prepared monomer mixture, deionized water and emulsifier sodium dodecyl sulfate are added into a three-necked flask in a weight ratio of 8:100:0.05-0.15, stirred, and nitrogen protection is passed through. The temperature is raised to 75°C, an initiator is added, and the reaction is performed for 8 hours, and the reaction is stopped; the amount of the initiator is 3 wt% of the total mass of the monomer; after the reaction is completed, centrifuge at 10000 rpm, remove the supernatant, add deionized water, ultrasonically disperse for 30 minutes, and then centrifuge again; repeat 3 times to remove unreacted monomers and other small molecular impurities; the washed polystyrene cross-linked nanospheres are redispersed in deionized water to prepare a dispersion with a concentration of 5 wt% for standby use; Step 2: Preparation of functional polystyrene nanospheres The polystyrene cross-linked nanosphere dispersion prepared in step 1 is dispersed in deionized water to prepare a 1wt% dispersion, and ammonium persulfate is dissolved in deionized water to prepare a 5wt% aqueous solution; pyrrole monomer and ammonium persulfate aqueous solution are added to the dispersion under stirring conditions, and the reaction is continued for 48 hours; wherein the molar ratio of pyrrole monomer to ammonium persulfate is 4:1; centrifuge at 10000 rpm using a centrifuge, remove the supernatant, add anhydrous ethanol, ultrasonically disperse for 30 minutes, and then centrifuge again; repeat 3 times to remove unreacted monomers and other small molecular impurities; the washed product is placed in a vacuum drying oven at 50°C and dried to obtain functional polystyrene nanospheres; Step 3: Preparation of polyethylene / functional polystyrene nanosphere composite insulating resin The polyethylene resin and the functional polystyrene nano-microspheres prepared in step 2 are weighed according to the ratio, and the components are added into an internal mixer for internal mixing to obtain a polyethylene / functional polystyrene nano-microsphere composite insulating resin.

6. The method for preparing a polyethylene / functional polystyrene nano-microsphere composite insulating resin according to claim 5, characterized in that: In step 1, the initiator is potassium persulfate.

7. The method for preparing a polyethylene / functional polystyrene nano-microsphere composite insulating resin according to claim 5, characterized in that: In step 3, the banburying temperature is 180-190°C, the banburying time is 6-10 min, and the banburying speed is 60 rpm.

8. Use of the polyethylene / functional polystyrene nano-microsphere composite insulating resin according to any one of claims 1 to 4 as an insulating material for high-voltage direct current transmission cables.