A lithium carbonate polymer composite material and preparation method thereof
By using carbon microspheres to load lithium carbonate in epoxy resin and modifying it with copper lignosulfonate, the problem of poor flame retardant effect of epoxy resin is solved, the mechanical and flame retardant properties of the composite material are improved, and a higher Thermal stability and impact resistance.
Patent Information
- Application Number
- CN202311601483.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-11-28
AI Technical Summary
The poor flame retardant effect of epoxy resin limits its application in composite materials, and the addition of high filler content will reduce the mechanical properties.
Carbon microspheres loaded with lithium carbonate are used as fillers, and are modified by copper lignosulfonate to improve the dispersion and compatibility of the fillers, thereby improving the flame retardant effect.
It improves the mechanical properties and flame retardant properties of the polymer, enhances the wear resistance and impact resistance of the composite material, and forms stable coke through the high thermal stability of the carbon microspheres and the cross-linking of copper oxide, which significantly improves the flame retardant effect.
Smart Images

Figure CN117624834B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material preparation, and specifically refers to a lithium carbonate polymer composite material and a preparation method thereof. Background Art
[0002] Epoxy resin has excellent mechanical properties, adhesive properties, electrical insulation properties, dimensional stability, etc. It is easy to process and has low cost, which makes epoxy resin widely used in composite materials. However, like most polymer materials, epoxy resin composed of C, H, and O is extremely flammable and easy to cause fire, which greatly limits the application range of epoxy resin. Therefore, it is very important to flame retardant it. At present, the most common method to improve flame retardancy is to add inorganic additives, but the addition of high-content fillers will deteriorate the mechanical properties of composite materials. At the same time, the type and properties of fillers also greatly affect the flame retardant effect of composite materials.
[0003] The existing technology currently has the following main problems: epoxy resin has poor flame retardant effect. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a lithium carbonate polymer composite material and a preparation method thereof. In order to solve the problem of poor flame retardant effect of epoxy resin, the present invention proposes to load lithium carbonate as a filler by carbon microspheres to improve the mechanical properties and flame retardant properties of the polymer, and at the same time use copper lignin sulfonate to modify the filler to improve the dispersibility and compatibility of the filler and improve the flame retardant effect.
[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: The present invention proposes a lithium carbonate polymer composite material and a preparation method thereof, wherein the lithium carbonate polymer composite material comprises the following components in parts by weight: 20-35 parts of lithium carbonate composite filler, 60-80 parts of epoxy resin, 50-75 parts of curing agent, and 20-40 parts of diluent.
[0006] Furthermore, the preparation method of the lithium carbonate composite filler comprises the following steps:
[0007] (1) lithium acetate dihydrate was added to 50 mL of deionized water, stirred until completely dissolved, carbon microspheres were added, stirred for 10-20 min, and ultrasonically treated to obtain a mixed solution;
[0008] (2) filtering the mixed solution of step (1), drying at 80° C. for 6-8 h, grinding through a 200-mesh sieve, and calcining at 500° C. for 3-4 h under vacuum conditions to obtain a lithium carbonate composite material;
[0009] (3) Take the composite material of step (2) and add it into 100 mL of deionized water, ultrasonically treat it, add 50 mL of sodium lignin sulfonate aqueous solution, stir for 20-40 min, slowly add 50 mL of copper chloride solution, continue to stir for 1-2 h after the addition is completed, filter and wash the obtained product, dry it at 80° C. for 8-10 h, and obtain lithium carbonate composite filler.
[0010] Furthermore, in step (1), the mass ratio of lithium acetate dihydrate to carbon microspheres is 1:2-3.
[0011] Furthermore, in step (1), the power of the ultrasonic treatment is 100 W and the time is 10-15 min.
[0012] Furthermore, in step (3), the mass fraction of the composite material in deionized water is 2-3%.
[0013] Furthermore, in step (3), the power of the ultrasonic treatment is 200 W and the time is 5-10 min.
[0014] Furthermore, in step (3), the concentration of the sodium lignin sulfonate aqueous solution is 5 g / L.
[0015] Furthermore, in step (3), the concentration of the copper chloride solution is 0.05 mol / L.
[0016] The present invention provides a method for preparing a lithium carbonate polymer composite material, which specifically comprises the following steps:
[0017] The epoxy resin is added into an organic solvent, a lithium carbonate composite filler is added, the mixture is stirred evenly, a curing agent is added and cured, and a lithium carbonate high molecular polymer composite material is obtained.
[0018] The beneficial effects achieved by the present invention are as follows:
[0019] The invention uses carbon microspheres loaded with lithium carbonate as fillers to improve the mechanical properties and flame retardant properties of polymers, and uses copper lignin sulfonate to modify the fillers, thereby improving the dispersibility and compatibility of the fillers and improving the flame retardant effect. The carbon microspheres have the advantages of small particle size, high thermal stability and good chemical stability. When added to polymers as fillers, the strength and rigidity of the composite material can be improved, making the composite material more wear-resistant and impact-resistant. At the same time, the carbon microspheres have a high surface area and a porous structure, and can be used as carriers to load lithium carbonate. The lithium carbonate slows down or inhibits the combustion process of the material by absorbing heat and releasing inert gas, thereby improving the flame retardant properties of the material. The copper lignin sulfonate is used to coat the carbon microsphere / lithium carbonate composite material, thereby improving the hydrophobicity of the carbon microsphere / lithium carbonate composite material, improving the dispersibility of the carbon microsphere / lithium carbonate composite material in a matrix and the compatibility with the matrix, and simultaneously improving the flame retardant effect of the carbon microsphere / lithium carbonate composite material. The copper oxide generated by the copper lignin sulfonate at high temperature can cross-link with the lignin sulfonate coke and the carbon microspheres to form highly stable coke, and the stable coke is conducive to improving the flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The thermal stability test results of the lithium carbonate polymer composite material of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0021] Figure 2 The tensile strength test results of the lithium carbonate polymer composite material of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.
[0022] Figure 3 This is a graph showing the impact strength test results of the lithium carbonate polymer composite material of Examples 1-3 of the present invention and Comparative Examples 1-2;
[0023] Figure 4 This is a scanning electron microscope image of the lithium carbonate composite filler described in Example 1 of the present invention.
[0024] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0027] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0028] Some of the materials involved in the examples are from the following sources:
[0029] The curing agent is methyltetrahydrophthalic anhydride, CasNo: 11070-44-3, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0030] The diluent was butyl glycidyl ether, CasNo: 2426-08-6, purchased from Aladdin Biochemical Technology Co., Ltd.
[0031] Example 1
[0032] A lithium carbonate macromolecular polymer composite material comprises the following components in parts by weight: 20 parts of lithium carbonate composite filler, 60 parts of epoxy resin, 50 parts of organic solvent and 20 parts of curing agent.
[0033] The preparation method of the lithium carbonate composite filler comprises the following steps:
[0034] (1) Add 1 g of lithium acetate dihydrate to 50 mL of deionized water, stir until completely dissolved, add 2 g of carbon microspheres, stir for 10 min, and perform ultrasonic treatment at a power of 100 W for 10 min to obtain a mixed solution;
[0035] (2) filtering the mixed solution in step (1), drying at 80° C. for 6 h, grinding through a 200-mesh sieve, and calcining at 500° C. for 3 h under vacuum conditions to obtain a lithium carbonate composite material;
[0036] (3) Take 2 g of the composite material of step (2) and add it to 100 mL of deionized water. Ultrasonic treatment is performed at a power of 200 W for 5 min. 50 mL of a 5 g / L sodium lignin sulfonate aqueous solution is added and stirred for 20 min. 50 mL of a 0.05 mol / L copper chloride solution is slowly added dropwise. After the addition is completed, stirring is continued for 1 h. The obtained product is filtered and washed, and dried at 80 ° C for 8 h. The lithium carbonate composite filler is obtained.
[0037] This embodiment provides a method for preparing a lithium carbonate polymer composite material, which specifically comprises the following steps:
[0038] The epoxy resin is added into an organic solvent, a lithium carbonate composite filler is added, the mixture is stirred evenly, a curing agent is added and cured, and a lithium carbonate high molecular polymer composite material is obtained.
[0039] Example 2
[0040] A lithium carbonate macromolecular polymer composite material comprises the following components in parts by weight: 35 parts of lithium carbonate composite filler, 80 parts of epoxy resin, 75 parts of organic solvent and 40 parts of curing agent.
[0041] The preparation method of the lithium carbonate composite filler comprises the following steps:
[0042] (1) 1 g of lithium acetate dihydrate was added to 50 mL of deionized water and stirred until completely dissolved, 3 g of carbon microspheres were added, stirred for 20 min, and ultrasonically treated at a power of 100 W for 15 min to obtain a mixed solution;
[0043] (2) filtering the mixed solution in step (1), drying at 80° C. for 8 h, grinding through a 200-mesh sieve, and calcining at 500° C. for 4 h under vacuum conditions to obtain a lithium carbonate composite material;
[0044] (3) Take 3 g of the composite material described in step (2) and add it to 100 mL of deionized water. Ultrasonic treatment is performed at a power of 200 W for 10 min. 50 mL of a 5 g / L sodium lignin sulfonate aqueous solution is added and stirred for 40 min. 50 mL of a 0.05 mol / L copper chloride solution is slowly added dropwise. After the addition is completed, stirring is continued for 2 h. The obtained product is filtered and washed, and dried at 80 ° C for 10 h. The lithium carbonate composite filler is obtained.
[0045] This embodiment provides a method for preparing a lithium carbonate polymer composite material, and the preparation method is carried out with reference to Example 1.
[0046] Example 3
[0047] A lithium carbonate macromolecular polymer composite material comprises the following components in parts by weight: 30 parts of lithium carbonate composite filler, 70 parts of epoxy resin, 65 parts of organic solvent and 30 parts of curing agent.
[0048] The preparation method of the lithium carbonate composite filler comprises the following steps:
[0049] (1) 1 g of lithium acetate dihydrate was added to 50 mL of deionized water and stirred until completely dissolved, 2.5 g of carbon microspheres were added, stirred for 15 min, and ultrasonically treated at a power of 100 W for 13 min to obtain a mixed solution;
[0050] (2) filtering the mixed solution of step (1), drying at 80° C. for 7 h, grinding through a 200-mesh sieve, and calcining at 500° C. for 3.5 h under vacuum conditions to obtain a lithium carbonate composite material;
[0051] (3) Take 2.5 g of the composite material of step (2) and add it to 100 mL of deionized water. Ultrasonic treatment is performed at a power of 200 W for 8 min. 50 mL of a 5 g / L sodium lignin sulfonate aqueous solution is added and stirred for 30 min. 50 mL of a 0.05 mol / L copper chloride solution is slowly added dropwise. After the addition is completed, stirring is continued for 1.5 h. The obtained product is filtered and washed, and dried at 80 ° C for 9 h. The lithium carbonate composite filler is obtained.
[0052] This embodiment provides a method for preparing a lithium carbonate polymer composite material, and the preparation method is carried out with reference to Example 1.
[0053] Comparative Example 1
[0054] This comparative example provides a lithium carbonate polymer composite material and a preparation method thereof. The difference between the comparative example and Example 1 is that a composite filler not containing lithium carbonate is used instead of the lithium carbonate composite filler, and lithium acetate dihydrate is omitted in the process of preparing the lithium carbonate composite filler to obtain the composite filler not containing lithium carbonate, and the other components and component contents are the same as those in Example 1.
[0055] Comparative Example 2
[0056] This comparative example provides a lithium carbonate polymer composite material and a preparation method thereof. The difference between the comparative example and Example 1 is that the lithium carbonate composite filler does not contain copper lignin sulfonate, the preparation steps do not include step (3), and the remaining components and component contents are the same as those in Example 1.
[0057] Experimental example
[0058] 1. The thermal stability test of the lithium carbonate polymer composite materials prepared in Examples 1-3 of the present invention and Comparative Examples 1 and 2 is carried out as follows: Using a thermogravimetric analyzer, the temperature is raised to 800°C at a heating rate of 10°C / min in a nitrogen atmosphere, and the initial decomposition temperature T is recorded. 5% .
[0059] 2. The mechanical properties of the lithium carbonate polymer composite materials prepared in Examples 1-3 of the present invention and Comparative Examples 1 and 2 were tested. The specific method was based on GB / T2567-2008, and the mechanical properties were tested using a universal material testing machine.
[0060] 3. The surface morphology of the lithium carbonate composite filler described in Example 1 was observed using a scanning electron microscope.
[0061] Results Analysis
[0062] Figure 1 The thermal stability test results of the lithium carbonate polymer composite material of Examples 1-3 of the present invention and Comparative Examples 1-2 are shown in the figure. As shown in the figure, the T 5% The T of Comparative Example 1 is 346℃, 349℃, and 351℃ respectively. 5% is 311°C, and the T 5% The temperature is 305°C. It can be seen from Example 1 and Comparative Examples 1 and 2 that adding lithium carbonate and performing copper lignin sulfonate modification can improve the thermal stability of the composite material.
[0063] Figure 2 This is a graph showing the tensile strength test results of the lithium carbonate polymer composite materials of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, the tensile strengths of Examples 1-3 are 65 MPa, 63 MPa, and 66 MPa, respectively, the tensile strength of Comparative Example 1 is 28 MPa, and the tensile strength of Comparative Example 2 is 60 MPa. It can be seen from Example 1 and Comparative Example 1 that the addition of lithium carbonate as a filler can improve the tensile strength of the composite material.
[0064] Figure 3 This is a graph of the impact strength test results of the lithium carbonate polymer composite materials of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, the tensile strengths of Examples 1-3 are 32 MPa, 33 MPa, and 31 MPa, respectively, the tensile strength of Comparative Example 1 is 25 MPa, and the tensile strength of Comparative Example 2 is 27 MPa. It can be seen from Example 1 and Comparative Example 1 that adding lithium carbonate as a filler can improve the impact strength of the composite material.
[0065] Figure 4 This is the microscopic morphology of the lithium carbonate composite filler described in Example 1 of the present invention. The structure of the lithium carbonate composite filler is spherical, and the surface is coated with copper lignin sulfonate.
[0066] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0067] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A lithium carbonate polymer composite material, characterized in that: The invention comprises the following components in parts by weight: 20-35 parts of lithium carbonate composite filler, 60-80 parts of epoxy resin, 50-75 parts of organic solvent and 20-40 parts of curing agent; The preparation method of the lithium carbonate composite filler comprises the following steps: (1) Add lithium acetate dihydrate to 50 mL of deionized water, stir until completely dissolved, add carbon microspheres, stir for 10-20 min, and perform ultrasonic treatment to obtain a mixed solution; (2) filtering the mixed solution in step (1), drying at 80° C. for 6-8 h, grinding through a 200-mesh sieve, and calcining at 500° C. for 3-4 h under vacuum conditions to obtain a lithium carbonate composite material; (3) Take the composite material of step (2) and add it into 100 mL of deionized water, ultrasonically treat it, add 50 mL of sodium lignin sulfonate aqueous solution, stir for 20-40 min, slowly add 50 mL of copper chloride solution, continue to stir for 1-2 h after the addition is completed, filter and wash the obtained product, dry it at 80°C for 8-10 h, and obtain lithium carbonate composite filler.
2. A method for preparing the lithium carbonate polymer composite material according to claim 1, characterized in that: The method specifically comprises the following steps: adding epoxy resin into an organic solvent, adding a lithium carbonate composite filler, stirring evenly, adding a curing agent and curing to obtain a lithium carbonate high molecular polymer composite material.
3. The method for preparing the lithium carbonate polymer composite material according to claim 2, characterized in that: In step (1), the mass ratio of lithium acetate dihydrate to carbon microspheres is 1:2-3.
4. The method for preparing the lithium carbonate polymer composite material according to claim 3, characterized in that: In step (1), the power of the ultrasonic treatment is 100 W and the time is 10-15 min.
5. The method for preparing the lithium carbonate polymer composite material according to claim 4, characterized in that: In step (3), the mass fraction of the composite material in deionized water is 2-3%.
6. The method for preparing the lithium carbonate polymer composite material according to claim 5, characterized in that: In step (3), the power of the ultrasonic treatment is 200 W and the time is 5-10 min.
7. The method for preparing the lithium carbonate polymer composite material according to claim 6, characterized in that: In step (3), the concentration of the sodium lignin sulfonate aqueous solution is 5 g / L.
8. The method for preparing the lithium carbonate polymer composite material according to claim 7, characterized in that: In step (3), the concentration of the copper chloride solution is 0.05 mol / L.