A high entropy alloy performance optimization method and a high performance CoCrFeNiMn high entropy alloy

By mixing cobalt powder, chromium powder, iron powder and manganese powder according to atomic ratios, and optimizing printing parameters using additive manufacturing processes, the problems of low thermal utilization rate and high accuracy requirements in traditional alloy preparation are solved, and high performance is achieved The preparation of CoCrFeNiMn high-entropy alloy reduces surface defects and improves hardness and corrosion resistance.

CN117626030BActive Publication Date: 2024-11-22SHEN ZHEN WAN ZHI DA XIN XI ZI XUN YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311359958.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-19
Publication Date
2024-11-22
Estimated Expiration
2043-10-19

AI Technical Summary

Technical Problem

In the preparation method of traditional high-temperature metal parts, alloy smelting leads to low thermal utilization rate and high process accuracy requirements during the metal process processing stage. Especially in the aerospace field, how to prepare CoCrFeNiMn high-entropy alloys with stable performance and few surface defects exist. challenge.

Method used

By mixing cobalt powder, chromium powder, iron powder and manganese powder according to atomic ratios and printing and forming using additive manufacturing technology, the printing power and scanning speed are optimized, and the SLM mode and argon atmosphere are adopted to reduce surface defects and improve hardness and corrosion resistance.

Benefits of technology

It has achieved the reduction of surface defects of high-entropy alloys, improved the hardness and corrosion resistance stability of CoCrFeNiMn high-entropy alloys, and reduced the complexity and accuracy requirements of the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117626030B_ABST
    Figure CN117626030B_ABST
Patent Text Reader

Abstract

The present invention provides a method for optimizing the performance of a high entropy alloy and a high-performance CoCrFeNiMn high entropy alloy, belonging to the technical field of high-temperature metal component smelting and processing. The method for optimizing the performance of a high entropy alloy provided by the present invention comprises the following steps: (1) mixing cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equiatomic ratio to obtain a mixed powder; (2) using an additive manufacturing process to print and shape the mixed powder obtained in the step (1) to obtain a high-performance CoCrFeNiMn high entropy alloy; the parameters of the additive manufacturing process in the step (2) are: printing power 100-300W, scanning speed 500-1100mm / s. The results of the embodiment show that the optimization method provided by the present invention can reduce the surface defects of the CoCrFeNiMn high entropy alloy and improve the hardness and corrosion resistance of the CoCrFeNiMn high entropy alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-temperature metal component smelting and processing, and in particular to a method for optimizing the performance of a high-entropy alloy and a high-performance CoCrFeNiMn high-entropy alloy. Background Art

[0002] High-performance CoCrFeNiMn high-entropy alloy has great prospects for application in industrial engineering due to its high temperature resistance and high hardness, especially in high-temperature areas such as high-temperature components of industrial equipment, aircraft engine nozzles, and welding hot nozzles.

[0003] The traditional method of preparing alloys is metal smelting. The smelted alloys need to be roughly processed by metalworking processes such as turning, cutting, milling, and filing, and then the processed parts in the previous step are assembled into a whole through welding. In this process, the heat utilization rate of alloy smelting is low, and the temperature requirements for the start-up and cooling process of the smelting furnace are very high; at the same time, the requirements for process accuracy in the metal processing stage are also very strict, especially for precision parts used in the aerospace field.

[0004] In comparison, using additive manufacturing to process parts will save a lot of tedious steps. Additive manufacturing is also called 3D printing. Computer three-dimensional graphics are then directly printed and formed by a 3D printer. This process for preparing high-entropy alloys has a very high application prospect. However, the additive manufacturing process is affected by printing power, scanning speed, layer thickness and line spacing. Among them, printing power and scanning speed have the greatest impact on the performance of the printed alloy. At the same time, due to the different alloy elements or the different proportions of elements, the applicable additive manufacturing parameters are also different, resulting in unstable performance of high-entropy alloys. Therefore, how to prepare a CoCrFeNiMn high-entropy alloy with stable performance and few surface defects has become a technical problem that needs to be solved in this field. Summary of the invention

[0005] The purpose of the present invention is to provide a method for optimizing the performance of a high entropy alloy and a high-performance CoCrFeNiMn high entropy alloy. The optimization method provided by the present invention can reduce the surface defects of the high entropy alloy and improve the hardness and corrosion resistance stability of the CoCrFeNiMn high entropy alloy.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for optimizing the performance of a high entropy alloy, comprising the following steps:

[0008] (1) mixing cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equal atomic ratio to obtain a mixed powder;

[0009] (2) using an additive manufacturing process to print and shape the mixed powder obtained in step (1) to obtain a high-performance CoCrFeNiMn high-entropy alloy;

[0010] The parameters of the additive manufacturing process in step (2) are: printing power 100-300W, scanning speed 500-1100mm / s.

[0011] Preferably, in step (1), the particle sizes of the cobalt powder, chromium powder, iron powder, nickel powder and manganese powder are independently 5 to 70 μm.

[0012] Preferably, the mode of the additive manufacturing process in step (2) is the SLM mode.

[0013] Preferably, the parameters of the additive manufacturing process in step (2) are: printing power 150-250 W, scanning speed 700-900 mm / s.

[0014] Preferably, the parameters of the additive manufacturing process in step (2) are: printing power 200 W, scanning speed 900 mm / s.

[0015] Preferably, the atmosphere of the additive manufacturing process in step (2) is an argon atmosphere.

[0016] The present invention provides a high-performance CoCrFeNiMn high-entropy alloy prepared by the optimization method described in the above technical solution.

[0017] The present invention provides a method for optimizing the performance of a high entropy alloy, comprising the following steps: (1) mixing cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equiatomic ratio to obtain a mixed powder; (2) using an additive manufacturing process to print and shape the mixed powder obtained in the step (1) to obtain a high-performance CoCrFeNiMn high-entropy alloy; the parameters of the additive manufacturing process in the step (2) are: a printing power of 100 to 300 W and a scanning speed of 500 to 1100 mm / s. The present invention mixes cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equiatomic ratio to prepare a high entropy alloy. Since the ratio of each element in the high entropy alloy is fixed, the difference in the additive manufacturing parameters applicable thereto due to the difference in alloying elements or the difference in the proportion of elements is eliminated; by optimizing the printing power and scanning speed in the additive manufacturing process, it is avoided that the high melting point element particles cannot be melted due to too low printing power, and the high entropy alloy cannot be formed due to too slow cooling and excessive temperature accumulation due to too high printing power, thereby reducing the surface defects of the high entropy alloy and improving the performance stability of the CoCrFeNiMn high entropy alloy. The results of the embodiment show that the optimization method provided by the present invention can reduce the surface defects of the CoCrFeNiMn high entropy alloy and improve the hardness and corrosion resistance of the CoCrFeNiMn high entropy alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A diagram of the connection structure of the sample to be tested when testing the alloy polarization curve of the high-performance CoCrFeNiMn high-entropy alloy prepared in Examples 1 to 14 of the present invention;

[0019] Figure 2 Alloy polarization curves of high-performance CoCrFeNiMn high-entropy alloys prepared in Examples 1 to 4 of the present invention;

[0020] Figure 3 Alloy polarization curves of high-performance CoCrFeNiMn high-entropy alloys prepared in Examples 5 to 8 of the present invention;

[0021] Figure 4 Alloy polarization curves of high-performance CoCrFeNiMn high-entropy alloys prepared in Examples 9 to 12 of the present invention;

[0022] Figure 5 Alloy polarization curves of high-performance CoCrFeNiMn high-entropy alloys prepared in Examples 2, 6, 10, 13 and 14 of the present invention;

[0023] Figure 6 Surface microstructure diagram of high performance CoCrFeNiMn high entropy alloy prepared in Examples 1 to 12 of the present invention;

[0024] Figure 7 A partial enlarged view of the surface features of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 2 of the present invention;

[0025] Figure 8 Schematic diagram of hardness testing using sampling point distribution on the alloy surface;

[0026] Fig. 9 This is a hardness distribution bar graph of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 11 of the present invention;

[0027] Fig.10 The uncorroded morphology and polarization-corroded morphology of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 2 and Example 14 of the present invention;

[0028] Fig.11 Polarization curves of polarization corrosion of high-performance CoCrFeNiMn high-entropy alloys prepared in Examples 2 and 14 of the present invention;

[0029] Fig.12 A schematic diagram of the optimal process window interval for preparing high-performance CoCrFeNiMn high-entropy alloy using an additive manufacturing process in the present invention;

[0030] Fig.13 This is a physical picture of the CoCrFeNiMn high entropy alloy prepared in Comparative Example 1. DETAILED DESCRIPTION

[0031] The present invention provides a method for optimizing the performance of a high entropy alloy, comprising the following steps:

[0032] (1) mixing cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equal atomic ratio to obtain a mixed powder;

[0033] (2) using an additive manufacturing process to print and shape the mixed powder obtained in step (1) to obtain a high-performance CoCrFeNiMn high-entropy alloy;

[0034] The parameters of the additive manufacturing process in step (2) are: printing power 100-300W, scanning speed 500-1100mm / s.

[0035] The present invention mixes cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equal atomic ratio to obtain a mixed powder. The present invention has no particular limitation on the specific sources of the cobalt powder, chromium powder, iron powder, nickel powder and manganese powder, and commercially available products known to those skilled in the art can be used.

[0036] In the present invention, the particle sizes of the cobalt powder, chromium powder, iron powder, nickel powder and manganese powder are independently preferably 5 to 70 μm, more preferably 10 to 50 μm, and further preferably 25 to 30 μm.

[0037] The present invention has no special limitation on the mixing method of the cobalt powder, chromium powder, iron powder, nickel powder and manganese powder, as long as the components can be mixed evenly.

[0038] After obtaining the mixed powder, the present invention uses an additive manufacturing process to print and shape the mixed powder to obtain a high-performance CoCrFeNiMn high-entropy alloy.

[0039] In the present invention, the equipment used in the additive manufacturing process is preferably the SLM-DLM280 equipment produced by Hangzhou Dedi Intelligent Technology Co., Ltd.

[0040] In the present invention, the mode of the additive manufacturing process is preferably an SLM mode (selective laser melting mode). The present invention adopts the above mode for printing and forming, which is convenient for controlling parameters in the printing and forming process, thereby regulating the properties of the high entropy alloy.

[0041] In the present invention, the parameters of the additive manufacturing process are: printing power 100-300W, scanning speed 500-1100mm / s, preferably: printing power 150-250W, scanning speed 700-900mm / s, more preferably: printing power 200W, scanning speed 900mm / s. The present invention optimizes the printing power and scanning speed in the additive manufacturing process, thereby avoiding the phenomenon that the high melting point element particles cannot be melted due to too low printing power, and at the same time avoiding the phenomenon that the high entropy alloy cannot be formed due to too slow cooling and excessive temperature accumulation due to too high printing power.

[0042] In the present invention, the layer thickness of the additive manufacturing process is preferably 20 μm; the line spacing of the additive manufacturing process is preferably 80 μm; and the spot diameter of the additive manufacturing process is preferably 80 μm. The present invention reduces the influence of these parameters on the performance of the high entropy alloy by controlling the layer thickness and line spacing of the additive manufacturing process.

[0043] In the present invention, the atmosphere of the additive manufacturing process is preferably an argon atmosphere. In the present invention, the argon atmosphere is preferably obtained by first evacuating the vacuum and then filling the argon. The present invention can prevent gases such as oxygen in the air from contacting the metal and causing oxidation by printing in an inert atmosphere, thereby further improving the performance of the high entropy alloy.

[0044] The present invention mixes cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equiatomic ratio to prepare a high entropy alloy. Since the ratio of each element in the high entropy alloy is fixed, the difference in the applicable additive manufacturing parameters due to the difference in alloy elements or the difference in the proportion of the elements is eliminated; by optimizing the printing power and the scanning speed in the additive manufacturing process, it is avoided that the high melting point element particles cannot be melted due to too low printing power, and the high entropy alloy cannot be formed due to too slow cooling and excessive temperature accumulation due to too high printing power, thereby reducing the surface defects of the high entropy alloy and improving the performance stability of the CoCrFeNiMn high entropy alloy.

[0045] The present invention provides a high-performance CoCrFeNiMn high-entropy alloy prepared by the optimization method described in the above technical solution. In the present invention, the atomic ratio of Co:Cr:Fe:Ni:Mn in the high-performance CoCrFeNiMn high-entropy alloy is preferably 1:1:1:1:1.

[0046] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] A method for optimizing the performance of a high entropy alloy comprises the following steps:

[0049] (1) mixing cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equiatomic ratio to obtain a mixed powder; the average particle size of the cobalt powder, chromium powder, iron powder, nickel powder and manganese powder is independently 25 μm;

[0050] (2) using an SLM-DLM280 device produced by Hangzhou Dedi Intelligent Technology Co., Ltd. to print and shape the mixed powder obtained in step (1) through an additive manufacturing process to obtain a high-performance CoCrFeNiMn high-entropy alloy;

[0051] In the step (2), the additive manufacturing process is in SLM mode, the atmosphere of the additive manufacturing process is argon atmosphere, and the parameters of the additive manufacturing process are: printing power 100 W, scanning speed 500 mm / s, layer thickness 20 μm, line spacing 80 μm, and spot diameter 80 μm.

[0052] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 1 is 10 mm*10 mm*2 mm, denoted as A 10-5 .

[0053] Example 2

[0054] The parameters of the additive manufacturing process in step (2) are: printing power 100 W, scanning speed 700 mm / s, and other conditions are the same as those in Example 1.

[0055] The high performance CoCrFeNiMn high entropy alloy prepared in Example 2 is denoted as A 10-7 .

[0056] Example 3

[0057] The parameters of the additive manufacturing process in step (2) are: printing power 100 W, scanning speed 900 mm / s, and other conditions are the same as those in Example 1.

[0058] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 3 is 10 mm*10 mm*2 mm, denoted as A 10-9 .

[0059] Example 4

[0060] The parameters of the additive manufacturing process in step (2) are: printing power 100 W, scanning speed 1100 mm / s, and other conditions are the same as those in Example 1.

[0061] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 4 is 10 mm*10 mm*2 mm, denoted as A 10-11 .

[0062] Example 5

[0063] The parameters of the additive manufacturing process in step (2) are: printing power 150 W, scanning speed 500 mm / s, and other conditions are the same as those in Example 1.

[0064] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 5 is 10 mm*10 mm*2 mm, denoted as A 15-5 .

[0065] Example 6

[0066] The parameters of the additive manufacturing process in step (2) are: printing power 150 W, scanning speed 700 mm / s, and other conditions are the same as those in Example 1.

[0067] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 6 is 10 mm*10 mm*2 mm, denoted as A 15-7 .

[0068] Example 7

[0069] The parameters of the additive manufacturing process in step (2) are: printing power 150 W, scanning speed 900 mm / s, and other conditions are the same as those in Example 1.

[0070] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 7 is 10 mm*10 mm*2 mm, denoted as A 15-9 .

[0071] Example 8

[0072] The parameters of the additive manufacturing process in step (2) are: printing power 150 W, scanning speed 1100 mm / s, and other conditions are the same as those in Example 1.

[0073] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 8 is 10 mm*10 mm*2 mm, denoted as A 15-11 .

[0074] Example 9

[0075] The parameters of the additive manufacturing process in step (2) are: printing power 200 W, scanning speed 500 mm / s, and other conditions are the same as those in Example 1.

[0076] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 9 is 10 mm*10 mm*2 mm, denoted as A 20-5 .

[0077] Example 10

[0078] The parameters of the additive manufacturing process in step (2) are: printing power 200 W, scanning speed 700 mm / s, and other conditions are the same as those in Example 1.

[0079] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 10 is 10 mm*10 mm*2 mm, denoted as A 20-7 .

[0080] Embodiment 11

[0081] The parameters of the additive manufacturing process in step (2) are: printing power 200 W, scanning speed 900 mm / s, and other conditions are the same as those in Example 1.

[0082] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 11 is 10 mm*10 mm*2 mm, denoted as A 20-9 .

[0083] Example 12

[0084] The parameters of the additive manufacturing process in step (2) are: printing power 200 W, scanning speed 1100 mm / s, and other conditions are the same as those in Example 1.

[0085] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 12 is 10 mm*10 mm*2 mm, denoted as A 20-11 .

[0086] Embodiment 13

[0087] The parameters of the additive manufacturing process in step (2) are: printing power 250 W, scanning speed 700 mm / s, and other conditions are the same as those in Example 1.

[0088] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 13 is 10 mm*10 mm*2 mm, denoted as A 25-7 .

[0089] Embodiment 14

[0090] The parameters of the additive manufacturing process in step (2) are: printing power 300 W, scanning speed 700 mm / s, and other conditions are the same as those in Example 1.

[0091] The size of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 14 is 10 mm*10 mm*2 mm, denoted as A 30-7 .

[0092] Comparative Example 1

[0093] The parameters of the additive manufacturing process in step (2) are: printing power 400 W, scanning speed 700 mm / s, and other conditions are the same as those in Example 1.

[0094] The size of the CoCrFeNiMn high entropy alloy prepared in Comparative Example 1 is 10 mm*10 mm*2 mm, denoted as A 40-7 .

[0095] The alloy polarization curves of the high performance CoCrFeNiMn high entropy alloys prepared in Examples 1 to 14 were tested by the following method:

[0096] 1) The surface of the high-performance CoCrFeNiMn high-entropy alloy was treated with 150#, 600#, 2000# and 3000# sandpaper in sequence to remove surface impurities, then cleaned with anhydrous ethanol, and finally rinsed with deionized water again to obtain an alloy sample;

[0097] 2) The alloy sample obtained in step 1) is electrically connected to a copper wire, and the connection portion between the copper wire and the alloy sample is sealed with epoxy resin, leaving only a 10 mm*10 mm working surface of the high entropy alloy sample (such as Figure 1 As shown), obtain the sample to be tested;

[0098] 3) preparing a 3.5 wt. % NaCl solution, and then performing a polarization curve test on the test sample obtained in step 2).

[0099] The alloy polarization curves of the high performance CoCrFeNiMn high entropy alloys prepared in Examples 1 to 4 are as follows: Figure 2 The alloy polarization curves of the high performance CoCrFeNiMn high entropy alloys prepared in Examples 5 to 8 are shown in Figure 3 The alloy polarization curves of the high performance CoCrFeNiMn high entropy alloys prepared in Examples 9 to 12 are shown in Figure 4 The alloy polarization curves of the high performance CoCrFeNiMn high entropy alloys prepared in Example 2, Example 6, Example 10, Example 13 and Example 14 are shown in Figure 5 shown.

[0100] Depend on Figures 2 to 5It can be seen that the corrosion resistance is not much different when the scanning speed is 700mm / s and the power is above 200W. When the power is reduced to 100W, the passivation interval becomes significantly shorter. The reduction in power affects the formation of certain strengthening phase crystal structures. With the increase of scanning speed, the corrosion resistance of the alloy sample shows a downward trend, and this decline becomes more obvious with the reduction of power. In addition to the quality of alloy particles, power and laser scanning speed have a great influence on the performance of alloy samples. Due to the differences in the properties of each element in the high entropy alloy CoCrFeNiMn alloy mixed particles, when the volume laser energy density (VE) is insufficient, the temperature distribution and solidification behavior inside the laser molten pool cannot meet the performance requirements of traditional smelting samples; the calculation formula of volume laser energy density (VE) is shown in Formula I:

[0101] VE=p / vhs Formula I

[0102] In formula I, VE is the volume laser energy density, p is the printing power, v is the scanning speed, h is the layer thickness, and s is the line spacing;

[0103] From formula I, we can see that: when the layer thickness h and line spacing s are the same, as the printing power decreases, the corresponding volume laser energy density decreases, and the corresponding internal temperature of the laser molten pool is too low, resulting in insufficient melting of relatively high melting point alloy particles; similarly, the bubbles rushed in by the laser jet will also remain inside the alloy due to the solidification behavior under too low temperature. The scanning speed v also has the same influence mechanism as the power, both of which affect the volume laser energy density during printing and thus affect the internal environment of the molten pool.

[0104] The surface characteristics of the high-performance CoCrFeNiMn high-entropy alloys prepared in Examples 1 to 12 were observed by the following method:

[0105] I. Using 150#, 600#, 2000# and 3000# sandpapers in sequence to treat the surface of the high-performance CoCrFeNiMn high-entropy alloy to remove surface impurities, then cleaning with anhydrous ethanol, and finally rinsing the surface again with deionized water to obtain an alloy sample;

[0106] II. The surface of the alloy sample obtained in step I is treated with polishing pastes of W3, W2.5, W2, W1.5, W1 and W0.5 in sequence to remove mechanical scratches on the surface, and then cleaned with anhydrous ethanol to remove metal debris and the polishing paste mixture on the surface. Finally, the alloy sample is placed in anhydrous ethanol for ultrasonic vibration for 3 minutes, and the surface is rinsed with deionized water after being taken out with tweezers. The surface is allowed to stand and dried with a hot hair dryer to remove debris and impurities remaining in cracks and gaps to obtain the alloy sample to be tested;

[0107] III. The alloy sample obtained in step II is placed under an electron microscope to observe the surface defect distribution. The results are as follows: Figure 6 shown.

[0108] Depend on Figure 6 It can be seen that the distribution of the number of surface defects of the alloy samples changes regularly with the change of the alloy preparation process.

[0109] Figure 7 This is a partial enlarged view of the surface features of the high-performance CoCrFeNiMn high-entropy alloy prepared in Example 2. Figure 7 It can be seen that when the power is low, the laser molten pool temperature and cooling strategy will be affected, which is mainly manifested in the appearance of more voids and unmelted metal powder particles on the alloy surface.

[0110] The method for selecting the distribution of sampling points on the alloy surface (such as Figure 8 The hardness of the high performance CoCrFeNiMn high entropy alloy prepared in Example 11 was tested, and the test results are shown in Fig. 9 As shown. Figure 6 It can be seen that when testing the hardness of high-performance CoCrFeNiMn high-entropy alloy, the surface hardness of the high-entropy alloy changes with the distribution of surface defects (mainly unmelted element particles). The hardness of the alloy in the unmelted metal element area has increased significantly, while the Vickers hardness of the main part of the high-entropy alloy is distributed between 270 and 290. As the alloy printing power decreases and the scanning speed increases, the distribution of unmelted particles on the alloy surface will increase, and the number of unmelted areas in the alloy sampling points will increase, so that the overall hardness value of the alloy will also increase. However, this increase in hardness is not a favorable factor for the mechanical properties of the high-entropy alloy, but is due to defects caused by the alloy preparation not being in the optimal process range.

[0111] The corrosion resistance of the high-performance CoCrFeNiMn high-entropy alloys prepared in Example 2 and Example 14 was tested, and the test method was as follows:

[0112] ① using 150#, 600#, 2000# and 3000# sandpapers in sequence to treat the surface of the high-performance CoCrFeNiMn high-entropy alloy to remove surface impurities, then cleaning with anhydrous ethanol, and finally rinsing the surface again with deionized water to obtain an alloy sample;

[0113] ② Use polishing pastes with numbers of W3, W2.5, W2, W1.5, W1 and W0.5 in sequence to treat the surface of the alloy sample obtained in step I to remove mechanical scratches on the surface, then clean it with anhydrous ethanol to remove metal debris and the polishing paste mixture on the surface, finally place the alloy sample in anhydrous ethanol for ultrasonic vibration for 3 minutes, take it out with tweezers and rinse the surface with deionized water, let it stand and blow dry the surface with a hot hair dryer to remove debris and impurities remaining in cracks and gaps, and obtain an uncorroded sample;

[0114] ③ The uncorroded sample obtained in step ② is placed under an electron microscope to observe the surface morphology, and the results are recorded as A 10-7 and A 30-7 ;

[0115] ④ Electrically connect the uncorroded sample obtained in step ② to the copper wire, and seal the connection between the copper wire and the alloy sample with epoxy resin, leaving only a 10 mm*10 mm working surface of the high entropy alloy sample to obtain the alloy sample to be tested;

[0116] ⑤ Prepare a 3.5wt.% NaCl solution, and then subject the alloy sample to be tested obtained in step ④ to polarization corrosion at -2V to 0.5V for 150s, record the polarization curve of high entropy alloy corrosion, and then rinse with deionized water and dry in order to obtain a corrosion sample;

[0117] ⑥ The corrosion sample obtained in step ⑤ is placed under an electron microscope to observe the surface morphology, and the results are recorded as A 10-7a and A 30-7a .

[0118] The uncorroded morphology and polarization corrosion morphology of the high performance CoCrFeNiMn high entropy alloy prepared in Example 2 and Example 14 are shown in Fig.10 As shown in Figure 2, the polarization curve of high entropy alloy corrosion is as follows: Fig.11 As shown. Fig.10 and Fig.11 It can be seen that when the power is low and the scanning speed is too fast, there are too many surface defects and the corrosion is more serious, and the corresponding passivation interval of the polarization curve is also shorter. From this, it can be judged that surface defects are the direct cause of the corrosion resistance.

[0119] From the above analysis, it can be seen that when the volume laser energy density does not meet the melting temperature requirements of the high-performance CoCrFeNiMn high-entropy alloy, defects such as voids, cracks, and single metal particles will appear on the surface and inside the high-entropy alloy. At the same time, these defects will also affect the corrosion resistance, physical strength and other properties of the high-entropy alloy. The observation results can intuitively show that: with the increase of scanning speed, the number of distribution defects in the high-entropy alloy gradually increases; with the decrease of printing power, the number of distribution defects in the high-entropy alloy also increases. After the above analysis, the optimal process window range for preparing high-performance CoCrFeNiMn high-entropy alloy using additive manufacturing process is as follows: Fig.12 As shown. Fig.12 It can be seen that when the power exceeds 300W and the scanning speed is lower than 700mm / s, the solid structure of the sample is difficult to form; when the power is lower than 200W and the scanning speed is greater than 700mm / s, there will be too many surface defects and affect its performance.

[0120] The actual picture of the CoCrFeNiMn high entropy alloy prepared in Comparative Example 1 is as follows Fig.13 As shown. Fig.13 It can be seen that when the printing power is too high, the temperature will be too high, making it difficult to form the alloy sample.

[0121] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for optimizing the performance of a high entropy alloy, comprising the following steps: (1) mixing cobalt powder, chromium powder, iron powder, nickel powder and manganese powder in an equal atomic ratio to obtain a mixed powder; (2) using an additive manufacturing process to print and shape the mixed powder obtained in step (1) to obtain a high-performance CoCrFeNiMn high-entropy alloy; In the step (1), the particle sizes of the cobalt powder, chromium powder, iron powder, nickel powder and manganese powder are independently 25 to 30 μm; The mode of the additive manufacturing process in step (2) is the SLM mode; the parameters of the additive manufacturing process in step (2) are: printing power 200W, scanning speed 900mm / s; the layer thickness of the additive manufacturing process is 20μm; the line spacing of the additive manufacturing process is 80μm; the spot diameter of the additive manufacturing process is 80μm; the atmosphere of the additive manufacturing process is argon atmosphere.

2. The optimization method according to claim 1, characterized in that: The atmosphere of the additive manufacturing process in step (2) is an argon atmosphere.

3. The high-performance CoCrFeNiMn high-entropy alloy prepared by the optimization method according to any one of claims 1 to 2.