A membrane material and its preparation method and application
By using the composite technology of thermoplastic polyurethane electrospinning membrane and vancomycin hydrochloride-modified carbon nanotubes in winter clothing materials, the shortcomings of existing materials in terms of warmth retention and antibacterial properties are solved, and the efficient absorption of sunlight is converted into Heat energy and significant antibacterial effect, suitable for winter clothing fabrics.
Patent Information
- Application Number
- CN202311670917.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-07
AI Technical Summary
Existing winter clothing materials are insufficient in terms of warmth retention and antibacterial properties, making it difficult to meet multiple functional requirements at the same time.
A composite material of thermoplastic polyurethane electrospinning membrane and vancomycin hydrochloride-modified carbon nanotubes is used. Through electrospinning technology and ultrasonic treatment, vancomycin hydrochloride-modified carbon nanotubes are evenly distributed on the surface of the thermoplastic polyurethane membrane to enhance antibacterial properties. performance and warmth.
It achieves significant heating of the membrane material within 20 minutes and excellent antibacterial properties, with an antibacterial rate of 97-98% and good warmth retention properties.
Smart Images

Figure CN117626637B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a membrane material and a preparation method and application thereof. Background Art
[0002] For winter clothing, warmth preservation, safety and protection are of vital importance. CN103203906A discloses a double-sided pearl velvet winter clothing fabric, comprising: an outer pearl velvet fabric layer, an intermediate windproof fabric layer arranged on the inner surface of the outer pearl velvet fabric layer, and an inner pearl velvet fabric layer arranged on the inner surface of the intermediate windproof fabric layer, the outer pearl velvet fabric layer comprises an outer bottom yarn layer and an outer velvet yarn layer, the inner pearl velvet fabric layer comprises an inner bottom yarn layer and an inner velvet yarn layer, the outer velvet yarn layer and the inner velvet yarn layer use yarns of different colors, have better warmth preservation and windproof performance, the front and back sides have the same style and different colors, and can be worn on both sides. CN107757004A discloses a clothing fabric, comprising an outer layer, an interlayer and a bottom layer, characterized in that the outer layer is a silk layer, the interlayer is a wool knitted layer, and the bottom layer is a non-woven fabric lining layer. The outer layer, middle layer and bottom layer are stacked and quilted into one in sequence. The outer silk layer is moisture-absorbent, easy to dry and comfortable; the interlayer wool knitted layer is thick and wear-resistant, suitable for winter; the bottom non-woven fabric lining layer is wrinkle-resistant, but has poor antibacterial properties.
[0003] As a common material for clothing fabrics, thermoplastic polyurethane (TPU) films are necessary to give the fabrics multiple functions such as warmth retention and antibacterial properties. Therefore, developing a film material with both warmth retention and antibacterial properties for use in the preparation of clothing fabrics is an urgent problem to be solved in the art. Summary of the invention
[0004] In view of the deficiencies of the prior art, an object of the present invention is to provide a membrane material, which can solve the problem of warmth preservation and antibacterial of winter clothing materials.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a membrane material, comprising a thermoplastic polyurethane electrospun membrane and vancomycin hydrochloride modified carbon nanotubes composited on the thermoplastic polyurethane electrospun membrane, wherein the raw materials for preparing the vancomycin hydrochloride modified carbon nanotubes comprise, by weight: 8-12 parts of carbon nanotubes, 1.8-2.2 parts of vancomycin hydrochloride, 95-110 parts of morpholineethanesulfonic acid, 380-420 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 180-220 parts of N-hydroxysuccinimide.
[0007] Preferably, the weight proportion of the carbon nanotubes is 8-12 parts, for example, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, and specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0008] Preferably, the weight portion of the vancomycin hydrochloride is 1.8-2.2 parts, for example, it can be 1.8 parts, 1.9 parts, 2 parts, 2.1 parts, 2.2 parts, and specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0009] Preferably, the weight parts of the morpholineethanesulfonic acid are 95-110 parts, for example, 95 parts, 98 parts, 100 parts, 105 parts, 110 parts, and specific points between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0010] Preferably, the weight proportion of the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 380-420 parts, for example, 380 parts, 390 parts, 400 parts, 410 parts, 420 parts, and specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0011] Preferably, the weight proportion of the N-hydroxysuccinimide is 180-220 parts, for example, 180 parts, 190 parts, 200 parts, 210 parts, 220 parts, and specific values between the above values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific values included in the range.
[0012] The minimum inhibitory concentration of carbon nanotubes is 25-50g / mL, while the minimum inhibitory concentration of carbon nanotubes modified with Vancomycin hydrochloride is 0.1-1mg / mL, so the membrane material has good antibacterial properties. In principle, the antibacterial properties of the carbon nanotube film modified with Vancomycin hydrochloride are relatively good, mainly because the carbon nanotubes modified with Vancomycin hydrochloride have a secondary sterilization function. The longitudinal size of the carbon nanotubes is nanometer-scale, and the axial size is micrometer-scale. Some bacteria fall on the radial direction of the modified carbon nanotubes and are killed by the carbon nanotubes, while the bacteria that fall on the axial direction are killed by Vancomycin hydrochloride, so the membrane material has good antibacterial properties. Carbon nanotubes are easy to agglomerate, but they are easily dispersed after being modified with Vancomycin hydrochloride and ultrasound, and are evenly distributed on the surface of TPU, so the specific surface area is large and the heat preservation and heat storage function is excellent.
[0013] Preferably, the mass ratio of the thermoplastic polyurethane electrospinning membrane to the vancomycin hydrochloride modified carbon nanotubes is 100:(1-3).
[0014] Preferably, the raw materials for preparing the membrane material further include, by weight: 380-420 parts of solvent.
[0015] Preferably, the weight proportion of the solvent is 380-420, for example, 380, 390, 400, 410, 420, and specific values between the above values. Due to space limitations and for simplicity, the present invention no longer exhaustively lists the specific values included in the range.
[0016] Preferably, the solvent comprises any one of N,N-dimethylformamide, water or tetrahydrofuran, or a combination of at least two thereof.
[0017] In a second aspect, the present invention provides a method for preparing the membrane material according to the first aspect, the preparation method comprising:
[0018] S1: mixing carbon nanotubes, vancomycin hydrochloride, morpholineethanesulfonic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide to obtain vancomycin hydrochloride modified carbon nanotubes; electrospinning thermoplastic polyurethane to obtain a thermoplastic polyurethane electrospinning membrane;
[0019] S2: mixing the vancomycin hydrochloride modified carbon nanotubes obtained in step S1 with the thermoplastic polyurethane electrospinning membrane, and performing ultrasound to obtain the membrane material.
[0020] Preferably, the preparation method specifically comprises:
[0021] (1) mixing carbon nanotubes and a solvent, and subjecting the mixture to ultrasound to obtain a carbon nanotube dispersion; mixing thermoplastic polyurethane and the solvent, and subjecting the mixture to stirring and electrostatic spinning to obtain a thermoplastic polyurethane electrospinning membrane;
[0022] (2) mixing the carbon nanotube dispersion obtained in step (1), vancomycin hydrochloride, morpholineethanesulfonic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring and drying to obtain vancomycin hydrochloride modified carbon nanotubes;
[0023] (3) The thermoplastic polyurethane electrospinning membrane obtained in step (1), the vancomycin hydrochloride modified carbon nanotubes obtained in step (2) and a solvent are mixed, and ultrasonicated and dried to obtain the membrane material.
[0024] Preferably, the temperature of the ultrasound in step (1) is 40-60°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0025] Preferably, the ultrasound time in step (1) is 28-32 min, for example, 28 min, 29 min, 30 min, 31 min, 32 min, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0026] Preferably, the stirring time in step (1) is 6-10 h, for example, it can be 6 h, 7 h, 8 h, 9 h, 10 h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0027] Preferably, the stirring temperature in step (1) is 50-70°C, for example, it can be 50°C, 55°C, 60°C, 65°C, 70°C, and specific values between the above-mentioned points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0028] Preferably, the electrospinning rate of step (1) is 1-3 mL / h, for example, it can be 1 mL / h, 1.5 mL / h, 2 mL / h, 2.5 mL / h, 3 mL / h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0029] Preferably, the voltage of the electrospinning in step (1) is 1-20 kV, for example, it can be 1 kV, 3 kV, 5 kV, 8 kV, 10 kV, 15 kV, 18 kV, 20 kV, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0030] Preferably, the electrospinning time in step (1) is 2-5 h, for example, 2 h, 3 h, 4 h, 5 h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0031] Preferably, the stirring temperature in step (2) is 20-30°C, for example, it can be 20°C, 22°C, 25°C, 28°C, 30°C, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0032] Preferably, the stirring time in step (2) is 9-12 h, for example, it can be 9 h, 10 h, 11 h, 12 h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0033] Preferably, the drying time in step (2) is 1-3 h, for example, it can be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0034] Preferably, the drying temperature in step (2) is 35-40°C, for example, it can be 35°C, 36°C, 37°C, .8°C, 39°C, 40°C, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the said range.
[0035] Preferably, step (2) further includes centrifugation and washing steps after the drying.
[0036] Preferably, the centrifugation time is 2-4h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0037] Preferably, the washing comprises washing with morpholineethanesulfonic acid.
[0038] Preferably, the cleaning is performed 2-5 times, for example, 2 times, 3 times, 4 times, or 5 times.
[0039] Preferably, the temperature of the ultrasound in step (3) is 40-60°C, for example, it can be 40°C, 45°C, 50°C, 55°C, 60°C, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0040] Preferably, the ultrasonic time in step (3) is 50-70 min, for example, it can be 50 min, 55 min, 60 min, 65 min, 70 min, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0041] Preferably, the drying temperature in step (3) is 30-40°C, for example, it can be 30°C, 32°C, 35°C, 38°C, 40°C, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0042] Preferably, the drying time in step (3) is 1-3 h, for example, it can be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0043] Vancomycin hydrochloride modified carbon nanotubes are compounded onto a thermoplastic polyurethane electrospinning membrane by an ultrasonic method. The mechanism is as follows: Ultrasonic waves will cause cavitation bubbles to form in the liquid. When they hit the carbon nanotubes, the cavitation bubbles will deform or even break. The broken cavitation bubbles will generate high-intensity airflow or shock waves, thereby generating a large thrust and even high energy to partially melt the thermoplastic polyurethane electrospinning membrane, causing the carbon nanotubes to be deposited on the surface of the thermoplastic polyurethane electrospinning membrane.
[0044] The preparation of thermoplastic polyurethane electrospinning membrane is as follows: TPU is added to a mixed solution of DMF (N, N-dimethylformamide) and THF (tetrahydrofuran), stirred to form a solution with good fluidity, and set aside. The solution is electrospun at a voltage of 15 kV.
[0045] Vancomycin hydrochloride modified carbon nanotubes: carbon nanotubes are added to water, ultrasonicated, and then MES (morpholineethanesulfonic acid), EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride) and NHS (N-hydroxysuccinimide) are added to the dispersion of carbon nanotubes, stirred at room temperature, and then vancomycin hydrochloride is added to the above solution, continuously stirred, followed by centrifugation, washing several times with MES buffer solution, and drying.
[0046] The membrane material was prepared as follows: vancomycin hydrochloride-modified carbon nanotubes were added to a measuring cup containing water, and then a thermoplastic polyurethane electrospun membrane (1 cm × 1.5 cm) was placed in the measuring cup. The measuring cup was then placed under the probe of an ultrasonic cell crusher, ultrasonicated, and the membrane was taken out, stirred, and dried.
[0047] In a third aspect, the present invention provides a use of the membrane material as described in the first aspect in fabrics for infant clothing.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The invention provides a membrane material, which comprises a thermoplastic polyurethane electrospun membrane and vancomycin hydrochloride modified carbon nanotubes composited on the thermoplastic polyurethane electrospun membrane, and realizes the two functions of absorbing sunlight and converting it into heat energy and antibacterial. The temperature rise value in 20 minutes is 59.15-59.17°C, the temperature difference in 20 minutes is 24.09-24.1°C, and the antibacterial rate (Staphylococcus aureus) is 97-98%. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a graph showing the results of the antibacterial performance test of the membrane material provided by the present invention. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0052] The experimental materials used in the embodiments and comparative examples of the present invention are as follows:
[0053] (1) Carbon nanotubes, Aladdin Reagent Company, brand number 308068-56-6;
[0054] (2) Vancomycin hydrochloride, manufacturer: Aladdin Reagent Company, brand number 1404-90-6;
[0055] (3) Thermoplastic polyurethane, manufacturer: BASF AG, brand number 1190A10.
[0056] Example 1
[0057] The present embodiment provides a membrane material, which includes a thermoplastic polyurethane electrospinning membrane and vancomycin hydrochloride modified carbon nanotubes composited on the thermoplastic polyurethane electrospinning membrane. The raw materials for preparing the vancomycin hydrochloride modified carbon nanotubes include, by weight: 10 parts of DMF, 10 parts of THF, 10 parts of carbon nanotubes, 97.62 parts of MES (morpholineethanesulfonic acid), 400 parts of EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride) and 200 parts of NHS (N-hydroxysuccinimide), and 2 parts of vancomycin hydrochloride. The mass ratio of the thermoplastic polyurethane electrospinning membrane to the vancomycin hydrochloride modified carbon nanotubes is 100:2.
[0058] This embodiment also provides a method for preparing the membrane material, the method comprising:
[0059] (1) Add carbon nanotubes to water and ultrasonicate at 50°C for 30 min to obtain a dispersion of carbon nanotubes; add TPU to a mixed solution of DMF and THF and stir at 60°C for 8 h to obtain a solution with good fluidity. The solution is electrospun at a voltage of 15 kV to obtain a thermoplastic polyurethane electrospinning membrane at an electrospinning rate of 2 mL / h to obtain a thermoplastic polyurethane electrospinning membrane;
[0060] (2) adding MES, EDC and NHS to the carbon nanotube dispersion, stirring at room temperature for 10 min, then adding vancomycin hydrochloride to the above solution, stirring continuously for 10 h, then centrifuging for 180 min (3 h), washing with MES buffer solution 3 times, and drying in an oven at 37 ° C for 120 min (2 h) to obtain vancomycin hydrochloride modified carbon nanotubes;
[0061] (3) Vancomycin hydrochloride modified carbon nanotubes were added to a measuring cup of water, and then a thermoplastic polyurethane electrospun membrane (1 cm×1.5 cm) was placed in the measuring cup, and then the measuring cup was placed under the probe of an ultrasonic cell disruptor and ultrasonicated at 50° C. for 60 min. The membrane was taken out, stirred and cleaned for 3 h, and placed in an oven at 37° C. for 120 min (2 h) to obtain the membrane material.
[0062] Example 2
[0063] The present embodiment provides a membrane material, which includes a thermoplastic polyurethane electrospinning membrane and vancomycin hydrochloride modified carbon nanotubes composited on the thermoplastic polyurethane electrospinning membrane. The raw materials for preparing the vancomycin hydrochloride modified carbon nanotubes include, by weight: 10 parts of DMF, 10 parts of THF, 10 parts of carbon nanotubes, 97.62 parts of MES (morpholineethanesulfonic acid), 400 parts of EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride) and 200 parts of NHS (N-hydroxysuccinimide), and 2.2 parts of vancomycin hydrochloride. The mass ratio of the thermoplastic polyurethane electrospinning membrane to the vancomycin hydrochloride modified carbon nanotubes is 100:2.2.
[0064] This embodiment also provides a method for preparing the membrane material, the method comprising:
[0065] (1) Add carbon nanotubes to water and ultrasonicate at 40°C for 30 min to obtain a dispersion of carbon nanotubes; add TPU to a mixed solution of DMF and THF and stir at 60°C for 8 h to obtain a solution with good fluidity. The solution is electrospun at a voltage of 20 kV to obtain a thermoplastic polyurethane electrospinning membrane at an electrospinning rate of 2 mL / h to obtain a thermoplastic polyurethane electrospinning membrane;
[0066] (2) adding MES, EDC and NHS to the carbon nanotube dispersion, stirring at room temperature for 10 min, then adding vancomycin hydrochloride to the above solution, stirring continuously for 10 h, then centrifuging for 180 min (3 h), washing with MES buffer solution 3 times, and drying in an oven at 37° C. for 180 min (3 h) to obtain vancomycin hydrochloride modified carbon nanotubes;
[0067] (3) Vancomycin hydrochloride modified carbon nanotubes were added to a measuring cup of water, and then a thermoplastic polyurethane electrospun membrane (1 cm×1.5 cm) was placed in the measuring cup, and then the measuring cup was placed under the probe of an ultrasonic cell disruptor and ultrasonicated at 50° C. for 60 min. The membrane was taken out, stirred and cleaned for 3 h, and placed in an oven at 37° C. for 120 min (2 h) to obtain the membrane material.
[0068] Comparative Example 1
[0069] The present comparative example provides a carbon nanotube-TPU membrane, and the preparation method of the carbon nanotube-TPU membrane is as follows: carbon nanotubes are added to water, and ultrasonicated at 50°C for 30 minutes to obtain a dispersion of carbon nanotubes; TPU is added to a mixed solution of DMF and THF, and stirred at 60°C for 8 hours to form a solution with good fluidity, and the solution is electrospun at a voltage of 15 kV to obtain a thermoplastic polyurethane electrospinning membrane, and the electrospinning rate is 2 mL / h to obtain a carbon nanotube-TPU membrane.
[0070] Comparative Example 2
[0071] This comparative example provides a PU film, and the preparation method of the PU film is as follows: TPU is added to a mixed solution of DMF and THF, and stirred at 60°C for 8 hours to form a solution with good fluidity. The solution is electrospun at a voltage of 15 kV to obtain a thermoplastic polyurethane electrospinning film, and the electrospinning rate is 2 mL / h to obtain a PU film.
[0072] The performance tests were performed on the membrane materials provided in Examples 1-2, the carbon nanotube-TPU membrane provided in Comparative Example 1, and the PU membrane provided in Comparative Example 2. The specific methods are as follows:
[0073] (1) Heating performance: T / GDBX 012-2019 "Technical requirements for functional clothing";
[0074] 20-minute temperature rise value = 20th minute temperature - initial temperature;
[0075] 20-minute temperature difference = test sample temperature at the 20th minute - control sample temperature at the 20th minute;
[0076] (2) Antibacterial properties: GB / T 20944.3-2008 “Evaluation of antibacterial properties of textiles Part 3: Oscillation method”;
[0077] Bacterial inhibition rate: Staphylococcus aureus ≥ 70% is qualified;
[0078] The performance tests were conducted on the membrane materials provided in Examples 1-2, the carbon nanotube-TPU membrane provided in Comparative Example 1, and the PU membrane provided in Comparative Example 2. The test results are shown in Table 1:
[0079] Table 1
[0080]
[0081] As shown in Table 1, when vancomycin is used to modify carbon nanotubes, excellent antibacterial properties are obtained, and the modified carbon nanotubes have excellent light absorption and heat storage properties. Figure 1 As shown, the first row shows the bacterial distribution effect after 2 hours, and the second row shows the bacterial distribution effect after 24 hours; from left to right are Comparative Example 2, Comparative Example 1 and Example 1.
[0082] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate a membrane material and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A membrane material, characterized in that: The membrane material comprises a thermoplastic polyurethane electrospinning membrane and vancomycin hydrochloride modified carbon nanotubes composited on the thermoplastic polyurethane electrospinning membrane, wherein the raw materials for preparing the vancomycin hydrochloride modified carbon nanotubes comprise, by weight: 8-12 parts of carbon nanotubes, 1.8-2.2 parts of vancomycin hydrochloride, 95-110 parts of morpholineethanesulfonic acid, 380-420 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 180-220 parts of N-hydroxysuccinimide; The mass ratio of the thermoplastic polyurethane electrospinning membrane to the vancomycin hydrochloride modified carbon nanotubes is 100:(1-3).
2. The membrane material according to claim 1, characterized in that The raw materials for preparing the vancomycin hydrochloride modified carbon nanotubes further include, by weight: 380-420 parts of solvent.
3. The membrane material according to claim 2, characterized in that The solvent includes any one of N,N-dimethylformamide, water or tetrahydrofuran, or a combination of at least two thereof.
4. A method for preparing a membrane material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: S1: mixing carbon nanotubes and a solvent, and performing ultrasound to obtain a dispersion of carbon nanotubes; mixing vancomycin hydrochloride, morpholineethanesulfonic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide with the dispersion of carbon nanotubes to obtain vancomycin hydrochloride modified carbon nanotubes; and performing electrostatic spinning on thermoplastic polyurethane to obtain a thermoplastic polyurethane electrospinning membrane; S2: mixing the vancomycin hydrochloride modified carbon nanotubes obtained in step S1 with the thermoplastic polyurethane electrospinning membrane, and performing ultrasound to obtain the membrane material.
5. The preparation method according to claim 4, characterized in that: The preparation method specifically comprises: (1) mixing carbon nanotubes and a solvent, and subjecting them to ultrasound to obtain a carbon nanotube dispersion; mixing thermoplastic polyurethane and a solvent, and subjecting them to stirring and electrostatic spinning to obtain a thermoplastic polyurethane electrospinning membrane; (2) mixing the carbon nanotube dispersion obtained in step (1), vancomycin hydrochloride, morpholineethanesulfonic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring and drying to obtain vancomycin hydrochloride modified carbon nanotubes; (3) The thermoplastic polyurethane electrospinning membrane obtained in step (1), the vancomycin hydrochloride modified carbon nanotubes obtained in step (2) and a solvent are mixed, and ultrasonicated and dried to obtain the membrane material.
6. The preparation method according to claim 5, characterized in that: The temperature of the ultrasound in step (1) is 40-60°C.
7. The preparation method according to claim 5, characterized in that: The ultrasonic treatment time in step (1) is 28-32 minutes.
8. The preparation method according to claim 5, characterized in that: The stirring time in step (1) is 6-10 h.
9. The preparation method according to claim 5, characterized in that: The stirring temperature in step (1) is 50-70°C.
10. The preparation method according to claim 5, characterized in that: The electrospinning rate in step (1) is 1-3 mL / h.
11. The preparation method according to claim 5, characterized in that: The voltage of the electrospinning in step (1) is 1-20 kV.
12. The preparation method according to claim 5, characterized in that: The electrospinning time in step (1) is 2-5 hours.
13. The preparation method according to claim 5, characterized in that: The stirring temperature in step (2) is 20-30°C.
14. The preparation method according to claim 5, characterized in that: The stirring time in step (2) is 9-12 h.
15. The preparation method according to claim 5, characterized in that: The drying time in step (2) is 1-3 h.
16. The preparation method according to claim 5, characterized in that: The drying temperature in step (2) is 35-40°C.
17. The preparation method according to claim 5, characterized in that: Step (2) further includes centrifugation and washing steps after the drying.
18. The preparation method according to claim 17, characterized in that: The centrifugation time is 2-4 h.
19. The preparation method according to claim 17, characterized in that: The cleaning includes cleaning with morpholineethanesulfonic acid.
20. The preparation method according to claim 17, characterized in that: The cleaning is performed 2-5 times.
21. The preparation method according to claim 5, characterized in that: The temperature of the ultrasound in step (3) is 40-60°C.
22. The preparation method according to claim 5, characterized in that: The ultrasonic treatment time in step (3) is 50-70 minutes.
23. The preparation method according to claim 5, characterized in that: The drying temperature in step (3) is 30-40°C.
24. The preparation method according to claim 5, characterized in that: The drying time in step (3) is 1-3 hours.
25. Use of the membrane material according to any one of claims 1 to 3 in fabrics for infant clothing.
Citation Information
Patent Citations
Double-face pearl-cashmere winter clothing fabric
CN103203906A
Clothing fabric
CN107757004A
Modified polyamide reverse osmosis membrane with chemically grafted GO (graphene oxide) on surface and preparation method of modified polyamide reverse osmosis membrane
CN108176246A
Multi-response shape memory polyurethane material as well as preparation method and application thereof
CN112239593A
Length-based carbon nanotube ladders
US20200200706A1