A bismuth sulfide / MIL-88A (Fe) composite catalyst and its application in degradation of organic pollutants
Through the synergistic effect of bismuth sulfide/MIL-88A(Fe) composite catalyst and persulfate in the photocatalytic coupling system, the problem of low degradation efficiency of a single photocatalytic system is solved, and efficient degradation of refractory organic pollutants is achieved. In particular, the 87.03% degradation rate of dimethyl phthalate was significantly improved.
Patent Information
- Application Number
- CN202311592638.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-11-27
AI Technical Summary
The existing technology is difficult to efficiently degrade the refractory organic pollutant dimethyl phthalate, especially when using a single photocatalytic system, the recombination rate of photogenerated electrons and holes is high, which reduces its photocatalytic efficiency, and MIL- Application of 88A(Fe) and Bi2S3 composite catalyst in photocatalytic coupling persulfate activation technology.
Using bismuth sulfide/MIL-88A(Fe) composite catalyst, MIL-88A(Fe) acts synergistically with Bi2S3 and persulfate under light irradiation to improve photocatalytic oxidation activity and degrade phthalic acid The dimethyl ester method includes reacting MIL-88A(Fe) with bismuth nitrate pentahydrate and thiourea to form a Bi2S3/MIL-88A(Fe) composite catalyst, and apply it in a photocatalytic coupled persulfate system.
The degradation rate of dimethyl phthalate by potassium hydrogen persulfate in conjunction with light was significantly improved. The degradation rate reached 87.03% after 2 hours, which was much higher than the effect of single catalyst and single persulfate treatment.
Smart Images

Figure CN117643922B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sewage treatment, and in particular to a bismuth sulfide / MIL-88A (Fe) composite catalyst and application thereof in degrading organic pollutants. Background Art
[0002] Dimethyl phthalate (DMP) is one of the most representative refractory organic pollutants among phthalates. Compared with other phthalates, it has the highest hydrophilicity and is widely used in various industrial productions, such as pesticides, cosmetics, and lubricants. DMP is a flammable liquid, highly toxic, non-volatile and non-degradable. It is an endocrine disruptor and can induce cancer when in excessive amounts. It has now been included in the blacklist of environmental priority pollutants by countries around the world. Conventional methods for treating DMP take a long time and cannot be completely degraded. It is urgent to find a method for efficiently treating DMP pollutants.
[0003] Photocatalytic coupling with persulfate activation is a new water treatment process that is expected to become a new strategy for the efficient removal of difficult-to-degrade pollutants. In this coupling technology, the synergistic effect between light, catalysts and persulfate can be effectively developed and utilized, greatly improving the oxidation performance of the treatment process. In recent years, metal-organic frameworks (MOFs), as a new type of photocatalyst, have also been used in the photocatalytic synergistic persulfate oxidation process to remove difficult-to-degrade pollutants.
[0004] Since some MOFs are composed of transition metals and oxygen-containing ligands, the coordination of transition metals with the oxygen of the ligands produces metal oxide clusters within MOFs, which can exhibit photocatalytic activity. MIL-88A(Fe) has the advantages of high specific surface area, good light absorption performance, good stability and easy preparation, making it a photocatalyst with broad application prospects. Bi2S3 is an excellent photocatalytic material with a wide spectral response range and high quantum efficiency, but due to its narrow band gap, photogenerated electrons and holes are more likely to recombine, which is not conducive to the transfer of charge to the semiconductor surface for redox reactions to degrade pollutants. Therefore, it is necessary to explore a way to improve the photocatalytic properties of Bi2S3.
[0005] The disadvantage of a single photocatalytic system is that the recombination rate of photogenerated electrons and holes is high, which reduces its photocatalytic efficiency. In order to solve this problem, some researchers use persulfate to improve the overall photocatalytic oxidation activity. Studies have shown that under light irradiation, a large number of conduction band electrons on the surface of the photocatalyst will be captured by persulfate, slowing down the recombination of electrons and holes and improving the generation efficiency of hydroxyl radicals; more importantly, the capture of electrons by persulfate will produce a large number of strongly oxidizing sulfate radicals and hydroxyl radicals, attacking organic pollutants, thereby improving the oxidation capacity of the system. At present, there is no report on the use of MIL-88A (Fe) and Bi2S3 composite as a catalyst for photocatalytic coupling persulfate activation technology to degrade dimethyl phthalate. Summary of the invention
[0006] In view of the above-mentioned prior art, the purpose of the present invention is to provide a bismuth sulfide / MIL-88A(Fe) composite catalyst (Bi2S3 / MIL-88A(Fe) composite catalyst) and its application in degrading organic pollutants.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] In a first aspect of the present invention, a bismuth sulfide / MIL-88A(Fe) composite catalyst is provided, wherein the bismuth sulfide / MIL-88A(Fe) composite catalyst is prepared by the following method:
[0009] (1) adding MIL-88A(Fe) to ethylene glycol, performing ultrasonic dispersion for 5-15 minutes, adding bismuth nitrate pentahydrate to obtain liquid A; adding thiourea to N,N-dimethylformamide to obtain liquid B;
[0010] (2) Add liquid B to liquid A, stir evenly, react at 140-180° C. for 10-14 hours, cool after the reaction, collect the precipitate, wash the precipitate with N,N-dimethylformamide and ethanol in turn, and dry to obtain a bismuth sulfide / MIL-88A (Fe) composite catalyst.
[0011] Preferably, in step (1), the mass ratio of MIL-88A(Fe), bismuth nitrate pentahydrate and thiourea is (0.2-0.3):(0.2-0.3):(0.1~0.2).
[0012] Preferably, the MIL-88A(Fe) is prepared by the following method:
[0013] Ferric chloride hexahydrate and fumaric acid are respectively added into deionized water to obtain a ferric chloride hexahydrate solution and a fumaric acid solution; the fumaric acid solution is added into the ferric chloride hexahydrate solution, stirred evenly, reacted at 100-120° C. for 5-7 hours, cooled after the reaction, and the precipitate is collected, washed with deionized water, and dried to obtain MIL-88A(Fe).
[0014] Preferably, the mass ratio of the ferric chloride hexahydrate to the fumaric acid is (0.3-0.4):(0.1-0.2).
[0015] The above-mentioned bismuth sulfide / MIL-88A (Fe) composite catalyst is used in degrading organic pollutants in wastewater.
[0016] The above-mentioned bismuth sulfide / MIL-88A (Fe) composite catalyst is used in the photocatalytic coupling persulfate degradation of dimethyl phthalate.
[0017] A method for photocatalytically coupling persulfate to degrade dimethyl phthalate comprises the following steps:
[0018] A bismuth sulfide / MIL-88A (Fe) composite catalyst is added to a dimethyl phthalate solution and stirred to form a mixture; persulfate is added to the mixture to form a reaction system; and then a light source is turned on to irradiate the reaction system to degrade the dimethyl phthalate in the solution.
[0019] Preferably, the final concentration of the bismuth sulfide / MIL-88A(Fe) composite catalyst in the system is 0.1-1 g / L, the final concentration of the persulfate is 0.5-5 mmol / L, and the final concentration of dimethyl phthalate in the reaction system is 5-20 mg / L.
[0020] Beneficial effects of the present invention:
[0021] 1. The present invention prepares a Bi2S3 / MIL-88A(Fe) composite catalyst, and through the synergistic effect between MIL-88A(Fe) and Bi2S3, the degradation rate of dimethyl phthalate by potassium persulfate (PMS) and light is significantly improved.
[0022] 2. The present invention provides a method for photocatalytically coupling persulfate to degrade dimethyl phthalate. Through the simultaneous action of light, Bi2S3 / MIL-88A(Fe) composite catalyst and persulfate, efficient degradation of dimethyl phthalate is achieved. The degradation rate of dimethyl phthalate is 87.03% after 2 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1: SEM image of the Bi2S3 / MIL-88A(Fe) composite catalyst prepared in Example 1;
[0024] Figure 2 : XRD pattern of the Bi2S3 / MIL-88A(Fe) composite catalyst prepared in Example 1;
[0025] Figure 3 : Comparison of the degradation of dimethyl phthalate under different treatment conditions. DETAILED DESCRIPTION
[0026] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0027] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.
[0028] The Bi2S3 used in the present invention is prepared by the following method:
[0029] 0.2425g of bismuth nitrate pentahydrate was dissolved in 15mL of ethylene glycol and stirred magnetically to dissolve, which was recorded as solution 1; 0.17125g of thiourea was dissolved in 15mL of N,N-dimethylformamide and stirred magnetically to dissolve, which was recorded as solution 2. Solution 2 was added to solution 1 and stirred magnetically for 1 hour. The mixed solution was transferred into a 100mL polytetrafluoroethylene-lined stainless steel autoclave and heated in an oven at 160°C for 12 hours. After the reaction, the temperature of the autoclave was naturally cooled to room temperature, and the precipitate was collected; the precipitate was washed several times with N,N-dimethylformamide and ethanol in turn, and then placed in an oven at 60°C for 12 hours to obtain Bi2S3 powder.
[0030] Example 1: Preparation of Bi2S3 / MIL-88A(Fe) composite catalyst
[0031] (1) Preparation of MIL-88A(Fe):
[0032] 1) adding 0.35 g of ferric chloride hexahydrate to 5 mL of deionized water, stirring magnetically to dissolve, to obtain a ferric chloride hexahydrate solution; adding 0.14 g of fumaric acid to 20 mL of deionized water, stirring magnetically to dissolve, to obtain a fumaric acid solution;
[0033] 2) adding the fumaric acid solution to the ferric chloride hexahydrate solution, stirring magnetically for 1 hour to obtain a mixed solution, transferring the mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and heating it in an oven at 110° C. for 6 hours; after the reaction, naturally cooling the temperature of the autoclave to room temperature, collecting the precipitate, washing the precipitate with deionized water several times, and then placing it in an oven at 60° C. for 12 hours to obtain MIL-88A (Fe) powder.
[0034] (2) Preparation of Bi2S3 / MIL-88A(Fe) composite catalyst
[0035] 1) 0.27583 g of the above MIL-88A (Fe) was added to 15 mL of ethylene glycol, and ultrasonically dispersed for 10 minutes to make it uniformly dispersed, and 0.2425 g of bismuth nitrate pentahydrate was added to obtain liquid A; 0.17125 g of thiourea was added to 15 mL of N, N-dimethylformamide, and magnetically stirred for 30 minutes to obtain liquid B;
[0036] 2) Liquid B was added to liquid A, and the mixture was stirred magnetically for 1 hour. The mixed solution was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and heated in an oven at 160°C for 12 hours. After the reaction, the temperature of the autoclave was naturally cooled to room temperature, and the precipitate was collected. The precipitate was washed with N,N-dimethylformamide and ethanol several times in sequence, and then placed in an oven at 60°C for 12 hours to obtain a composite catalyst, which was recorded as Bi2S3 / MIL-88A(Fe).
[0037] Figure 1 This is a SEM image of the Bi2S3 / MIL-88A(Fe) composite catalyst prepared in Example 1, taken by a scanning electron microscope, model TESCAN MIRA LMS from Czech Republic. Figure 1 It can be seen that Bi2S3 particles are attached to MIL-88A(Fe), indicating that the Bi2S3 / MIL-88A(Fe) composite catalyst was successfully synthesized.
[0038] Figure 2 The XRD pattern of the Bi2S3 / MIL-88A(Fe) composite catalyst prepared in Example 1 was tested by an X-ray diffractometer, the instrument model was British Malvern Panalytical Empyrean, the test range was 5-90°, and the scanning speed was 10° / min. Figure 2 It can be seen from the XRD spectrum of the composite material that the characteristic diffraction peaks of MIL-88A(Fe) and Bi2S3 exist at the same time, indicating that the Bi2S3 / MIL-88A(Fe) composite catalyst was successfully synthesized.
[0039] Application example: Dimethyl phthalate degradation experiment
[0040] The experiment has 11 treatment groups:
[0041] The specific steps of treatment 1 (Bi2S3 / MIL-88A+PMS+light) are:
[0042] 10 mg of Bi2S3 / MIL-88A(Fe) composite catalyst was weighed and added to a 30 mL quartz tube; 10 mg / L of dimethyl phthalate was prepared, 30 mL of which was measured with a measuring cylinder and added to the quartz tube, the quartz tube was placed in a photocatalytic reactor, and magnetic stirring was performed for 30 minutes to allow the system to reach adsorption-desorption equilibrium; potassium persulfate was then added to make its final concentration in the system be 2 mmol / L, and a light source was turned on to irradiate the reaction system to degrade the dimethyl phthalate in the solution.
[0043] The specific steps of treatment 2 (Bi2S3+PMS+light) are:
[0044] Weigh 10 mg of Bi2S3 catalyst and add it to a 30 mL quartz tube; prepare 10 mg / L dimethyl phthalate, use a measuring cylinder to measure 30 mL and add it to the quartz tube, put the quartz tube into a photocatalytic reactor, and stir it magnetically for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then add potassium persulfate to make its final concentration in the system 2 mmol / L, turn on the light source to irradiate the reaction system, and degrade the dimethyl phthalate in the solution.
[0045] The specific steps of treatment 3 (MIL-88A+PMS+light) are:
[0046] 10 mg of MIL-88A (Fe) catalyst was weighed and added to a 30 mL quartz tube; 10 mg / L dimethyl phthalate was prepared, 30 mL was measured with a measuring cylinder and added to the quartz tube, the quartz tube was placed in a photocatalytic reactor, and magnetic stirring was performed for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then potassium persulfate was added to make its final concentration in the system 2 mmol / L, and a light source was turned on to irradiate the reaction system to degrade dimethyl phthalate in the solution.
[0047] The specific steps of treatment 4 (Bi2S3+light) are:
[0048] Weigh 10 mg of Bi2S3 catalyst and add it to a 30 mL quartz tube; prepare 10 mg / L dimethyl phthalate, use a measuring cylinder to measure 30 mL and add it to the quartz tube, put the quartz tube into a photocatalytic reactor, and stir it magnetically for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then turn on the light source to irradiate the reaction system to degrade the dimethyl phthalate in the solution.
[0049] The specific steps for treatment 5 (MIL-88A + light) are:
[0050] 10 mg of MIL-88A (Fe) catalyst was weighed and added to a 30 mL quartz tube; 10 mg / L dimethyl phthalate was prepared, 30 mL was measured with a measuring cylinder and added to the quartz tube, the quartz tube was placed in a photocatalytic reactor, and magnetic stirring was performed for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then a light source was turned on to irradiate the reaction system to degrade the dimethyl phthalate in the solution.
[0051] The specific steps of treatment 6 (Bi2S3 / MIL-88A+light) are:
[0052] Weigh 10 mg of Bi2S3 / MIL-88A(Fe) composite catalyst and add it to a 30 mL quartz tube; prepare 10 mg / L dimethyl phthalate, measure 30 mL with a measuring cylinder and add it to the quartz tube, put the quartz tube into a photocatalytic reactor, and stir it magnetically for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then turn on the light source to irradiate the reaction system to degrade the dimethyl phthalate in the solution.
[0053] The specific steps of treatment 7 (Bi2S3 / MIL-88A+PMS) are:
[0054] 10 mg of Bi2S3 / MIL-88A(Fe) composite catalyst was weighed and added to a 30 mL quartz tube; 10 mg / L dimethyl phthalate was prepared, 30 mL was measured with a measuring cylinder and added to the quartz tube, the quartz tube was placed in a photocatalytic reactor, and magnetic stirring was performed for 30 minutes to allow the system to reach adsorption-desorption equilibrium; potassium persulfate was then added to make its final concentration in the system 2 mmol / L to degrade dimethyl phthalate in the solution.
[0055] The specific steps of processing 8 (Bi2S3+PMS) are:
[0056] Weigh 10 mg of Bi2S3 catalyst and add it to a 30 mL quartz tube; prepare 10 mg / L dimethyl phthalate, measure 30 mL with a measuring cylinder and add it to the quartz tube, put the quartz tube into a photocatalytic reactor, and stir it magnetically for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then add potassium persulfate to make its final concentration in the system 2 mmol / L to degrade dimethyl phthalate in the solution.
[0057] The specific steps of treatment 9 (MIL-88A+PMS) are:
[0058] 10 mg of MIL-88A (Fe) catalyst was weighed and added to a 30 mL quartz tube; 10 mg / L dimethyl phthalate was prepared, 30 mL was measured with a measuring cylinder and added to the quartz tube, the quartz tube was placed in a photocatalytic reactor, and magnetic stirring was performed for 30 minutes to allow the system to reach adsorption-desorption equilibrium; then potassium persulfate was added to make its final concentration in the system 2 mmol / L, and the dimethyl phthalate in the solution was degraded.
[0059] The specific steps of processing 10 (PMS) are:
[0060] Prepare 10 mg / L dimethyl phthalate, measure 30 mL with a measuring cylinder and add it to the quartz tube, put the quartz tube into a photocatalytic reactor, stir it magnetically for 30 minutes, and then add potassium persulfate to make its final concentration in the system 2 mmol / L to degrade dimethyl phthalate in the solution.
[0061] The specific steps of treatment 11 (PMS+light) are:
[0062] Prepare 10 mg / L dimethyl phthalate, measure 30 mL with a measuring cylinder and add it to the quartz tube, put the quartz tube into a photocatalytic reactor, stir it magnetically for 30 minutes, then add potassium persulfate to make its final concentration in the system 2 mmol / L, turn on the light source to irradiate the reaction system, and degrade the dimethyl phthalate in the solution.
[0063] The photocatalytic reactor used in the present invention is a multi-channel photocatalytic reaction system, model PL-SXE-8, and the light source used is a xenon lamp with a power of 850W.
[0064] Sampling method: Take 1 mL of degradation solution from treatments 1-11 at regular intervals under magnetic stirring, add it to a liquid phase vial that has been pre-added with 500 μL of HPLC methanol through an organic filter; use HPLC to determine the content of dimethyl phthalate in the solution, and calculate the degradation rate, see Figure 3 and Table 1.
[0065] The degradation rates of dimethyl phthalate in treatments 1 to 11 after two hours of degradation are shown in Table 1.
[0066] Concentration ratio = C t / C0
[0067] Degradation rate (%) = (1-concentration ratio) × 100%
[0068] Among them, C t is the concentration of dimethyl phthalate when sampling at different degradation times, and C0 is the initial concentration of dimethyl phthalate.
[0069] Table 1 Degradation rate of dimethyl phthalate after 2h under different treatment conditions
[0070]
[0071]
[0072] Figure 3 From -30 minutes to 0 minutes, the light source was not turned on, potassium persulfate was not added, and only materials were added, in order to make the system reach adsorption-desorption equilibrium.
[0073] Depend on Figure 3 As shown in Table 1, in treatment 1, Bi2S3 / MIL-88A composite catalyst and potassium persulfate (PMS) were added to the reaction system at the same time and the light source was turned on for irradiation. After 2 hours, the degradation rate of dimethyl phthalate was 87.03%, which was significantly higher than that of other treatment groups. In treatment 11, potassium persulfate (PMS) was added to the reaction system at the same time and the light source was turned on for irradiation. After 2 hours, the degradation rate of dimethyl phthalate was 58.94%. In treatments 2-3, a single Bi2S3 catalyst and a single MIL-88A (Fe) catalyst and potassium persulfate (PMS) were selected and the light source was turned on for irradiation. The degradation rates after 2 hours were 26.35% and 23.68%, respectively; it is proved that the composite of MIL-88A (Fe) and Bi2S3 has a synergistic effect on improving the degradation rate of dimethyl phthalate by potassium persulfate (PMS) and light. The degradation rates of dimethyl phthalate in other systems with only persulfate added, systems with a single catalyst and coordinated light treatment, systems with a single catalyst and persulfate treated simultaneously, and systems with Bi2S3 / MIL-88A(Fe) composite catalyst and persulfate were all low; this indicates that only when light, Bi2S3 / MIL-88A(Fe) composite catalyst and persulfate act simultaneously can efficient degradation of dimethyl phthalate be achieved.
[0074] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. Application of a bismuth sulfide / MIL-88A (Fe) composite catalyst in photocatalytic coupling persulfate degradation of dimethyl phthalate, It is characterized in that The bismuth sulfide / MIL-88A (Fe) composite catalyst is prepared by the following method: (1) Add MIL-88A (Fe) to ethylene glycol, disperse by ultrasonic for 5-15 minutes, add bismuth nitrate pentahydrate to obtain liquid A; add thiourea to N,N-dimethylformamide to obtain liquid B; (2) Add liquid B to liquid A, stir evenly, and react at 140-180°C for 10-14 h. After the reaction, cool and collect the precipitate. Wash the precipitate with N,N-dimethylformamide and ethanol in turn, and dry to obtain a bismuth sulfide / MIL-88A(Fe) composite catalyst.
2. The use according to claim 1, It is characterized in that In step (1), the mass ratio of MIL-88A (Fe), bismuth nitrate pentahydrate and thiourea is (0.2-0.3): (0.2-0.3): (0.1~0.2).
3. The use according to claim 1, It is characterized in that The MIL-88A (Fe) is prepared by the following method: Ferric chloride hexahydrate and fumaric acid are respectively added into deionized water to obtain a ferric chloride hexahydrate solution and a fumaric acid solution; the fumaric acid solution is added into the ferric chloride hexahydrate solution, stirred evenly, reacted at 100-120° C. for 5-7 hours, cooled after the reaction, and the precipitate is collected, washed with deionized water, and dried to obtain MIL-88A (Fe).
4. The use according to claim 3, It is characterized in that The mass ratio of the ferric chloride hexahydrate to the fumaric acid is (0.3-0.4):(0.1-0.2).
5. A method for photocatalytically coupling persulfate to degrade dimethyl phthalate, It is characterized in that The following steps are involved: Adding bismuth sulfide / MIL-88A(Fe) composite catalyst to a dimethyl phthalate solution and stirring to form a mixture; adding persulfate to the mixture to form a reaction system; then turning on a light source to irradiate the reaction system to degrade the dimethyl phthalate in the solution; The bismuth sulfide / MIL-88A (Fe) composite catalyst is prepared by the following method: (1) Add MIL-88A (Fe) to ethylene glycol, disperse by ultrasonic for 5-15 minutes, add bismuth nitrate pentahydrate to obtain liquid A; add thiourea to N,N-dimethylformamide to obtain liquid B; (2) Add liquid B to liquid A, stir evenly, and react at 140-180°C for 10-14 h. After the reaction, cool and collect the precipitate. Wash the precipitate with N,N-dimethylformamide and ethanol in turn, and dry to obtain a bismuth sulfide / MIL-88A(Fe) composite catalyst.
6. The method according to claim 5, It is characterized in that In step (1), the mass ratio of MIL-88A (Fe), bismuth nitrate pentahydrate and thiourea is (0.2-0.3): (0.2-0.3): (0.1~0.2).
7. The method according to claim 5, It is characterized in that The MIL-88A (Fe) is prepared by the following method: Ferric chloride hexahydrate and fumaric acid are respectively added into deionized water to obtain a ferric chloride hexahydrate solution and a fumaric acid solution; the fumaric acid solution is added into the ferric chloride hexahydrate solution, stirred evenly, reacted at 100-120° C. for 5-7 hours, cooled after the reaction, and the precipitate is collected, washed with deionized water, and dried to obtain MIL-88A (Fe).
8. The method according to claim 7, It is characterized in that The mass ratio of the ferric chloride hexahydrate to the fumaric acid is (0.3-0.4):(0.1-0.2).
9. The method according to claim 5, It is characterized in that The final concentration of bismuth sulfide / MIL-88A(Fe) composite catalyst in the system is 0.1~1 g / L, the final concentration of persulfate is 0.5~5 mmol / L, and the final concentration of dimethyl phthalate in the reaction system is 5~20 mg / L.