Bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material and preparation method thereof

By simultaneously doping bismuth and bismuth sulfide in bismuth carbonate to form bismuth-bismuth sulfide heterostructure, the problem of Bi2O2CO3 insufficient response to ultraviolet light is solved, and the photocatalytic performance and degradation effect of the material are improved. It has wide application prospects.

CN115814830BActive Publication Date: 2024-11-19SHANDONG AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211439055.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-11-19
Estimated Expiration
2042-11-17

Smart Images

  • Figure CN115814830B_ABST
    Figure CN115814830B_ABST
Patent Text Reader

Abstract

The invention discloses a bismuth-bismuth carbonate-bismuth sulfide heterostructure photocatalytic material and a preparation method thereof, and belongs to the field of photocatalyst technology. The preparation method of the photocatalyst of the present invention comprises the following steps: adding DMF to a Na2S solution to obtain a first mixed solution; slowly adding the first mixed solution to a Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution; stirring the second mixed solution, and then reacting in a closed manner at 150-240°C for 12-48h, and after the reaction is completed, naturally cooling to room temperature, centrifuging the product, washing with water, washing with alcohol, and drying at room temperature to obtain a bismuth-bismuth carbonate-bismuth sulfide heterostructure photocatalytic material. The present invention uses bismuth and bismuth sulfide to dope and modify the bismuth carbonate photocatalytic material, solving the problem that the bismuth carbonate photocatalytic material is insufficiently responsive to ultraviolet light; and the preparation method of the bismuth-bismuth carbonate-bismuth sulfide heterostructure photocatalytic material of the present invention is simple, easy to mass produce, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalysts, and in particular to a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material and a preparation method thereof. Background Art

[0002] In the research of photocatalytic technology, semiconductor photocatalysts have always attracted much attention. Using visible light, which accounts for the largest proportion of the solar spectrum, to effectively degrade organic matter is one of the most promising technologies for solving energy problems. Photocatalytic degradation is an advanced oxidation process involving semiconductor photocatalysts and oxygen to generate free radicals. It has the characteristics of fast degradation speed and wide application range, and can reduce secondary pollution during the degradation process. Domestic and foreign studies have shown that catalytic oxidation technology has a good removal effect on PAEs in water. In the process of photocatalysis, the photocatalytic activity of the catalyst plays a vital role. Therefore, finding a photocatalytic activity with a broad-spectrum effect has become a research hotspot in this field.

[0003] Gradually, bismuth-based photocatalysts have appeared in people's field of vision. Due to their suitable bandgap width, low toxicity, and wide sources of raw materials for their preparation, they have become an ideal visible light catalytic material. However, due to the wide bandgap width and small absorption range of Bi2O2CO3, its photocatalytic activity is greatly limited, resulting in low photocatalytic efficiency. In order to overcome this shortcoming, people continue to explore various strategies and find that the photocatalytic activity of wide bandgap photocatalytic materials can be effectively improved by methods such as morphology adjustment, metal deposition or heterostructure construction. In addition, another strategy has attracted our attention, which is metal element doping. As a semi-metal, bismuth nanoparticles not only have an ultra-narrow band gap, but also have surface plasmon resonance (SPR) behavior. Therefore, Bi nanoparticles are often used to functionalize other bismuth-based photoactive nanomaterials to improve their photocatalytic activity.

[0004] However, no research has been conducted on Bi / Bi2O2CO3 / Bi2S3. In order to overcome the problem of insufficient response of bismuth oxycarbonate to ultraviolet light, and further improve the catalytic effect of heterojunctions containing bismuth oxycarbonate, the preparation method of heterojunctions containing bismuth oxycarbonate is simplified so that it can be more widely used. Summary of the invention

[0005] In view of the above-mentioned prior art, the purpose of the present invention is to provide a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material and a preparation method thereof. The present invention adopts bismuth and bismuth sulfide to dope and modify the bismuth oxycarbonate photocatalytic material, thereby solving the problem that the bismuth oxycarbonate photocatalytic material is insufficiently responsive to ultraviolet light; and the preparation method of the bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material of the present invention is simple, easy to mass produce, and has good application prospects.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] In a first aspect of the present invention, a method for preparing a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material is provided, comprising the following steps:

[0008] (1) adding sodium sulfide to deionized water to obtain a sodium sulfide solution; adding N,N-dimethylformamide (DMF) to the sodium sulfide solution to obtain a first mixed solution;

[0009] (2) adding Bi(NO3)3·5H2O to ethylene glycol to obtain a Bi(NO3)3·5H2O ethylene glycol solution; slowly adding the first mixed solution to the Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution;

[0010] (3) The second mixed solution is stirred, and then reacted in a sealed state at 150-240° C. for 12-48 hours. After the reaction is completed, the mixture is naturally cooled to room temperature, and the product is centrifuged, washed with water and alcohol, and dried at room temperature to obtain a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material.

[0011] Preferably, the molar ratio of Bi(NO3)3·5H2O to sodium sulfide is (1-5):(1-5).

[0012] Preferably, the stirring is magnetic stirring, and the stirring time is 15-60 min.

[0013] Preferably, the centrifugal temperature is 4-25°C, the centrifugal speed is 4000-12000 rpm, and the centrifugal time is 5-15 min.

[0014] The second aspect of the present invention provides a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material prepared by the above preparation method.

[0015] The third aspect of the present invention provides the use of the above-mentioned bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material in photocatalytic degradation of plasticizers.

[0016] In the above application, preferably, the plasticizer is BBP.

[0017] Beneficial effects of the present invention:

[0018] (1) At present, there is no research on Bi / Bi2O2CO3 / Bi2S3. The present invention synthesizes the ternary composite material by a one-step method, which has a simple process flow, is low in cost, and is easy for large-scale production.

[0019] (2) The Bi / Bi2O2CO3 / Bi2S3 heterojunction prepared by the present invention has been tested and found to have the following advantages: the optical properties of the prepared samples were verified by UV-Vis diffuse reflectance spectroscopy. After bismuth oxycarbonate was doped with Bi and bismuth sulfide, its light absorption capacity was greatly enhanced, the absorption band was broadened to the visible light range, and the photocatalytic performance of the product was significantly improved. The bismuth sulfide heterojunction can accelerate the separation of electrons and holes and prolong the life of photogenerated electrons or holes; bismuth nanoparticles have an ultra-narrow band gap and surface plasmon resonance (SPR) behavior, which can effectively improve the photocatalytic activity of the photocatalyst. Therefore, bismuth, bismuth oxycarbonate and bismuth sulfide can play a synergistic role, further improving the photocatalytic ability of the material and effectively degrading pollutants such as plasticizers. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XRD spectrum of the Bi / Bi2O2CO3 / Bi2S3 heterostructure photocatalytic material prepared in Example 2.

[0021] Figure 2 This is the SEM photograph of the Bi / Bi2O2CO3 / Bi2S3 heterostructure photocatalytic material prepared in Example 2.

[0022] Figure 3 These are the solid fluorescence characterization test results of the photocatalytic materials prepared in Example 2 and Comparative Example 1-Comparative Example 2.

[0023] Figure 4 This is a comparison chart of the degradation of the plasticizer BBP by the photocatalytic materials prepared in Example 2 and Comparative Examples 1 to 4. DETAILED DESCRIPTION

[0024] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0025] Terminology Note:

[0026] Room temperature: refers to the temperature of 15-25℃.

[0027] As mentioned above, due to the wide bandgap and small light absorption range of Bi2O2CO3, its photocatalytic activity is greatly limited, resulting in low photocatalytic efficiency. To solve this problem, the inventors prepared a bismuth oxycarbonate-bismuth sulfide heterostructure photocatalyst in previous research, which solved the problem of insufficient response of bismuth oxycarbonate to ultraviolet light as a photocatalytic material.

[0028] Regarding metal element doping, patent CN 108745393 A discloses a bismuth-bismuth carbonate heterostructure photocatalyst, which uses Bi(NO3)3·5H2O as a raw material and methanol as a solvent and a reducing agent. The produced bismuth-bismuth carbonate heterostructure photocatalyst is a single bismuth nanoparticle deposited on the surface of flaky bismuth carbonate, which solves the problem of insufficient response of bismuth carbonate to ultraviolet light as a photocatalytic material.

[0029] However, there is no report on the simultaneous doping modification of bismuth sulfide and bismuth. Based on this, the present invention conducts in-depth research on the simultaneous doping modification of bismuth sulfide and bismuth of bismuth oxycarbonate, and develops and designs a one-step method for synthesizing Bi / Bi2O2CO3 / Bi2S3 ternary composite materials.

[0030] In one embodiment of the present invention, a one-step method for synthesizing a Bi / Bi2O2CO3 / Bi2S3 ternary composite material is provided, comprising the following steps:

[0031] DMF is added to a Na2S solution to obtain a first mixed solution; the first mixed solution is slowly added to a Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution; the second mixed solution is stirred, and then a closed reaction is carried out at 150-240°C for 12-48 hours. After the reaction is completed, the mixture is naturally cooled to room temperature, the product is centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material.

[0032] In the synthesis method of the present invention, Bi(NO3)3·5H2O is used as a bismuth source, sodium sulfide is used as a sulfur source, and DMF and ethylene glycol are used as solvents and also as carbon sources and reducing agents. By the method of the present invention, bismuth oxycarbonate can be doped with bismuth sulfide and bismuth at the same time in one step. Moreover, experiments have shown that compared with doping with bismuth sulfide alone and doping with bismuth alone, doping with bismuth sulfide and bismuth at the same time can significantly improve the catalytic efficiency of the photocatalytic material and has a synergistic effect.

[0033] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.

[0034] The test materials used in the examples and comparative examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels. The experimental methods without detailed conditions are carried out according to conventional test methods or the operating instructions recommended by the supplier.

[0035] Embodiment 1:

[0036] 5 mmol of Bi(NO3)3·5H2O was added to 15 mL of ethylene glycol, stirred and dissolved to obtain a Bi(NO3)3·5H2O ethylene glycol solution. 3 mmol of Na2S was added to 35 mL of water, stirred and dissolved to obtain a Na2S solution.

[0037] 10 mL of DMF was added to the Na2S solution to obtain a first mixed solution, and the first mixed solution was slowly added to the Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution. The second mixed solution was placed on a magnetic stirrer for mechanical stirring for 30 min. The second mixed solution was transferred to a polytetrafluoroethylene liner, and the liner was placed in a reactor and kept warm for 24 h at 180°C for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material.

[0038] Embodiment 2:

[0039] 4 mmol of Bi(NO3)3·5H2O was added to 15 mL of ethylene glycol, stirred and dissolved to obtain a Bi(NO3)3·5H2O ethylene glycol solution. 3 mmol of Na2S was added to 35 mL of water, stirred and dissolved to obtain a Na2S solution.

[0040] 10 mL of DMF was added to the Na2S solution to obtain a first mixed solution, and the first mixed solution was slowly added to the Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution. The second mixed solution was placed on a magnetic stirrer for mechanical stirring for 30 min. The second mixed solution was transferred to a polytetrafluoroethylene liner, and the liner was placed in a reactor and kept warm for 24 h at 180°C for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material.

[0041] The XRD pattern of bismuth-bismuth carbonate-bismuth sulfide heterostructure photocatalytic material is shown in Figure 1 ,Depend on Figure 1 It can be seen that the bismuth-bismuth oxycarbonate-bismuth sulfide heterojunction is indeed prepared in this embodiment. Figure 2 The SEM photograph of the bismuth-bismuth oxycarbonate-bismuth sulfide prepared in this example is shown, and the structural state of the composite material can be clearly seen.

[0042] Embodiment 3:

[0043] 3 mmol of Bi(NO3)3·5H2O was added to 15 mL of ethylene glycol, stirred and dissolved to obtain a Bi(NO3)3·5H2O ethylene glycol solution. 3 mmol of Na2S was added to 35 mL of water, stirred and dissolved to obtain a Na2S solution.

[0044] 10 mL of DMF was added to the Na2S solution to obtain a first mixed solution, and the first mixed solution was slowly added to the Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution. The second mixed solution was placed on a magnetic stirrer and mechanically stirred for 30 min. The second mixed solution was transferred to a polytetrafluoroethylene liner, and the liner was placed in a reactor and kept warm at 160°C for 24 h for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material.

[0045] Comparative Example 1: Preparation of Bismuth Oxycarbonate Photocatalyst

[0046] 0.5 g of urea was added to deionized water, and after stirring to dissolve, 2.75 mmol of Bi(NO3)3·5H2O was added to the solution and mechanically stirred. After stirring, a mixed solution was obtained. The mixed solution was placed on a magnetic stirrer and mechanically stirred for 30 min. The mixed solution was transferred to a polytetrafluoroethylene liner, and the liner was placed in a reactor and kept warm at 200°C for 24 h for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth carbonate photocatalytic material.

[0047] Comparative Example 2: Preparation of Bismuth Sulfide Photocatalyst

[0048] 4 mmol of Bi(NO3)3·5H2O was added to 15 mL of water and stirred to dissolve to obtain a Bi(NO3)3·5H2O solution. 3 mmol of Na2S was added to 35 mL of water and stirred to dissolve to obtain a Na2S solution.

[0049] Slowly add the Na2S solution to the Bi(NO3)3·5H2O solution. Finally, place the mixed solution on a magnetic stirrer for mechanical stirring for 30 minutes. Transfer the mixed solution to a polytetrafluoroethylene liner, place the liner in a reactor and keep it warm at 180°C for 24 hours for reaction; after the reaction is completed, cool it naturally to room temperature, centrifuge the product, wash it with water, wash it with alcohol, and dry it at room temperature to obtain a bismuth sulfide heterostructure photocatalytic material.

[0050] Comparative Example 3: Preparation of Bismuth-Bicarbonate Photocatalyst

[0051] 2.425 g of Bi(NO3)3·5H2O was added to a mixed solution of 15 mL of methanol and 15 mL of deionized water. The mixed solution was transferred to a polytetrafluoroethylene liner, which was placed in a reactor and kept at 180°C for 12 h for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water and alcohol, and dried at room temperature to obtain a bismuth-bismuth carbonate heterostructure photocatalytic material.

[0052] Comparative Example 4: Preparation of Bismuth Oxycarbonate-Bismuth Sulfide Photocatalyst

[0053] 0.5 g of urea was added to deionized water, and after stirring to dissolve, 2.75 mmol of Bi(NO3)3·5H2O was added to the solution and mechanically stirred. After stirring, 3 mmol of sodium sulfide was added to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer and mechanically stirred for 30 min. The mixed solution was transferred to a polytetrafluoroethylene liner, and the liner was placed in a reactor and kept warm at 200°C for 24 h for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth carbonate-bismuth sulfide heterostructure photocatalytic material.

[0054] The solid fluorescence characterization test results of the photocatalytic materials prepared in Example 2 and Comparative Example 1-Comparative Example 2 are shown in Figure 2 ,Depend on Figure 2 It can be seen that the composite photocatalytic material has a lower fluorescence intensity than that of a single material, indicating that the formation of the bismuth-bismuth oxycarbonate-bismuth sulfide heterojunction effectively improves the separation efficiency of electrons and holes.

[0055] Application example: Application of composite photocatalyst to degrade organic pollutant butyl benzyl phthalate (BBP) under visible light

[0056] Take 50 mg of the photocatalyst prepared in Example 2 and Comparative Examples 1 to 4, place them in 100 mL beakers respectively, add 25 mL of ultrapure water, ultrasonicate for 20 min to make it evenly dispersed, take 25 mL of 20 mg / L BBP solution and add it to the uniform solution after ultrasonication to obtain a photocatalytic system of 10 mg / L BBP solution and 0.5 g / L catalyst. Place on a magnetic stirrer and stir. Place the beaker on a magnetic stirrer and conduct a dark reaction under stirring conditions to make the catalyst evenly dispersed in the system and reach adsorption equilibrium.

[0057] After the dark reaction (sampling 2 mL), the xenon lamp light source was turned on to conduct the visible light catalytic degradation experiment. During the photocatalytic reaction, 2 mL was sampled every 30 minutes, and the reaction time was 2 hours.

[0058] The centrifuge tube was centrifuged at 10,000 rpm for 5 min to separate the solid and liquid, and the catalyst was recovered. The liquid was filtered through a 0.45 μm filter head (organic system) and placed in a chromatographic bottle and stored at 4°C.

[0059] The prepared samples were subjected to high performance liquid chromatography to measure the pollutant concentration and to determine the degradation efficiency of the composite material. Figure 4 It can be seen that the catalyst prepared in Example 2 can effectively degrade BBP, and the residual rate of BBP after degradation is about 12%; the residual rates of bismuth carbonate prepared in Comparative Example 1 and bismuth sulfide prepared in Comparative Example 2 after degradation of BBP are about 80% and 58% respectively; the residual rates of bismuth-bismuth carbonate prepared in Comparative Example 3 and bismuth sulfide-bismuth carbonate prepared in Comparative Example 4 are about 55% and 43% respectively, which are 25% and 37% higher than the degradation effect of bismuth carbonate prepared in Comparative Example 1. The degradation effect of bismuth-bismuth carbonate-bismuth sulfide is about 68% higher than that of bismuth carbonate, which is higher than that of bismuth-bismuth carbonate and bismuth sulfide-bismuth carbonate. It can be seen that the bismuth-bismuth carbonate-bismuth sulfide heterostructure photocatalytic material prepared by the present invention can achieve effective degradation of plasticizers such as BBP.

[0060] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for degrading butyl benzyl phthalate using a composite photocatalyst, characterized in that: The following steps are involved: 50 mg of the composite photocatalyst was placed in a 100 mL beaker, 25 mL of ultrapure water was added, and the mixture was uniformly dispersed by ultrasonication for 20 min. 25 mL of 20 g / L butyl benzyl phthalate solution was added to the uniform solution after ultrasonication to obtain a photocatalytic system. The beaker was placed on a magnetic stirrer, and a dark reaction was carried out under stirring conditions to uniformly disperse the composite photocatalyst in the system and reach adsorption equilibrium. After the dark reaction, a xenon lamp light source was turned on to carry out visible light photocatalytic degradation. The composite photocatalyst is prepared by the following method: 4 mmol of Bi(NO3)3·5H2O was added to 15 mL of ethylene glycol, and stirred to dissolve to obtain a Bi(NO3)3·5H2O ethylene glycol solution. 3 mmol of Na2S was added to 35 mL of water, and stirred to dissolve to obtain a Na2S solution. 10 mL of DMF was added to the Na2S solution to obtain a first mixed solution, the first mixed solution was slowly added to the Bi(NO3)3·5H2O ethylene glycol solution to obtain a second mixed solution, the second mixed solution was placed on a magnetic stirrer for mechanical stirring for 30 min, the second mixed solution was transferred to a polytetrafluoroethylene liner, the liner was placed in a reactor and kept warm for 24 h at 180° C. for reaction; after the reaction was completed, it was naturally cooled to room temperature, the product was centrifuged, washed with water, washed with alcohol, and dried at room temperature to obtain a bismuth-bismuth oxycarbonate-bismuth sulfide heterostructure photocatalytic material.