A lithium-manganese-rich lithium-ion battery electrolyte and a preparation method thereof
By using a mixed solvent of cyclic carbonate and linear carbonate and tri-n-butylphosphorus tetrafluoroborate as electrolyte additives in lithium-ion batteries, a low-resistance interface film is formed, which solves the problem of electrode surface decomposition of lithium-rich manganese-based cathode materials. problem, significantly improving the cycle performance and rate performance of the battery, and extending the life of the battery.
Patent Information
- Application Number
- CN202311588400.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-11-27
AI Technical Summary
In existing lithium-ion batteries, the high charging cut-off voltage of lithium-rich manganese-based cathode materials causes the traditional electrolyte to decompose on the electrode surface, forming an uneven interface, hindering Li+ diffusion, reducing electrochemical performance, and accompanied by side reactions, weakening cycle life.
A mixed solvent of cyclic carbonate and linear carbonate is used as the organic solvent of the electrolyte, and tri-n-butylphosphorus tetrafluoroborate is added as an electrolyte additive to form a low-resistance interface film to hinder the oxidative decomposition of the electrolyte and protect the electrode material.
The cycle performance and rate performance of lithium-rich manganese-based electrodes are significantly improved, the cycle life of the battery is extended, and the increase in electrode interface impedance and side reactions are reduced.
Smart Images

Figure CN117650272B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion batteries, and in particular relates to a lithium-manganese-rich lithium ion battery electrolyte and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, and no memory effect. They are one of the most widely used electrochemical energy storage devices. In recent years, new energy electric vehicles driven by lithium-ion batteries have been vigorously developed. However, as the demand for electric vehicles for longer driving range gradually increases, the energy density requirements for lithium-ion batteries are also gradually increasing. As an important component of lithium-ion batteries, cathode materials directly determine the energy density of lithium-ion batteries. However, the actual specific capacity of existing commercial cathode materials is less than 200 mAh g -1 The energy density of lithium-ion full batteries assembled based on these positive electrode materials is low, which makes it difficult to meet the demand of electric vehicles for longer driving range.
[0003] The discharge capacity of lithium-rich manganese-based cathode materials is as high as 300 mAh g -1 (2~4.8 V), which is much higher than the current commercial lithium-ion battery cathode materials. It is considered to be the ideal choice for the next generation of high energy density lithium-ion batteries. It is also the lithium-ion battery energy density that exceeds 400Wh kg -1 Even 500 Wh kg -1 However, in practical applications, its high charge cutoff voltage of 4.8 V relative to metallic lithium causes the traditional carbonate-based electrolyte to decompose severely on the surface of the lithium-rich manganese-based cathode, forming an uneven, unstable and unprotected cathode-electrolyte interface, which hinders the Li + Diffusion and reduced electrochemical performance. At the same time, it is accompanied by side reactions such as the release of lattice oxygen, the dissolution of transition metals, especially manganese, and irreversible structural transformation, which seriously weaken its electrochemical performance. Therefore, it is urgent to design and develop electrolytes suitable for lithium-rich manganese-based lithium-ion batteries, change the electrode surface morphology, protect the electrode materials, and improve the cycle life of lithium-rich manganese-based lithium-ion batteries. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a lithium-rich manganese-based lithium-ion battery electrolyte and a preparation method thereof, which can change the electrode surface morphology, protect the electrode material, and improve the cycle life of the lithium-rich manganese-based lithium-ion battery.
[0005] The technical solution of the present invention is:
[0006] A lithium-manganese-rich lithium-ion battery electrolyte comprises a basic electrolyte and an electrolyte additive, wherein the basic electrolyte is a lithium salt and an electrolyte organic solvent, and the special features thereof are:
[0007] The electrolyte additive structural formula is:
[0008]
[0009] The electrolyte organic solvent is a mixed solvent of cyclic carbonate solvent ethylene carbonate and linear carbonate solvents ethyl methyl carbonate and diethyl carbonate, wherein the volume ratio of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate is 1:1:1;
[0010] Electrolyte additives account for 0.5%-3% of the mass of the basic electrolyte.
[0011] Furthermore, the lithium salt is one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium tetrafluorooxalatophosphate.
[0012] Furthermore, the concentration of lithium salt in the electrolyte is 0.9 mol L -1 -1.1 mol L -1 .
[0013] Furthermore, the electrolyte additive accounts for 1% of the mass of the basic electrolyte.
[0014] Furthermore, the lithium salt is lithium hexafluorophosphate.
[0015] A method for preparing the above-mentioned lithium-rich manganese-based lithium-ion battery electrolyte comprises the following steps:
[0016] (1) Preparation of basic electrolyte
[0017] Ethylene carbonate, ethyl methyl carbonate and diethyl carbonate are uniformly mixed, and molecular sieves are used to purify and remove impurities and water, and lithium salt is added to obtain a basic electrolyte;
[0018] (2) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0019] The electrolyte additive is added to the basic electrolyte to obtain a lithium-rich manganese-based lithium-ion battery electrolyte.
[0020] Beneficial effects of the present invention:
[0021] The use of tri-n-butylphosphonium tetrafluoroborate as an electrolyte additive can be oxidized on the surface of the lithium-rich manganese-based electrode before the solvent, forming a low-impedance interface film, which effectively hinders the further oxidative decomposition of the electrolyte, protects the electrode material, alleviates the increase in electrode interface impedance, and reduces the side reactions between the lithium-rich manganese-based electrode and the electrolyte, thereby significantly improving the cycle performance of the lithium-rich manganese-based electrode, and the rate performance of the lithium-rich manganese-based lithium-ion battery is effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The figure is a comparison diagram of the LSV curves of the electrolytes of Comparative Example 1 and Example 2;
[0023] Figure 2 This is a comparison chart of the cycle performance of lithium-rich manganese-based batteries using the electrolytes of Comparative Example 1 and Example 2 at 1 C;
[0024] Figure 3 This is a comparison diagram of electrochemical impedance of lithium-rich manganese-based batteries using the electrolytes of Comparative Example 1 and Example 2 after 200 cycles at 1 C;
[0025] Figure 4 The figure is a comparison chart of the rate performance of lithium-rich manganese-based batteries using the electrolytes of Comparative Example 1 and Example 2. DETAILED DESCRIPTION
[0026] The present invention can be implemented in many different forms and is not limited to the embodiments described herein. The present invention is further described below in conjunction with embodiments.
[0027] Example 1
[0028] (1) Preparation of organic solvent for electrolyte
[0029] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0030] (2) Preparation of basic electrolyte
[0031] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain a basic electrolyte;
[0032] (3) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0033] Add tri-n-butylphosphonium tetrafluoroborate ( ) electrolyte additive, wherein the amount of the electrolyte additive is 0.5% of the mass of the basic electrolyte to obtain a lithium-rich manganese-based lithium-ion battery electrolyte.
[0034] Example 2
[0035] (1) Preparation of organic solvent for electrolyte
[0036] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0037] (2) Preparation of basic electrolyte
[0038] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain a basic electrolyte;
[0039] (3) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0040] Tri-n-butylphosphonium tetrafluoroborate electrolyte additive is added to the basic electrolyte prepared in step (2), wherein the amount of the electrolyte additive is 1% of the mass of the basic electrolyte, to obtain a lithium-rich manganese-based lithium ion battery electrolyte.
[0041] Example 3
[0042] (1) Preparation of organic solvent for electrolyte
[0043] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0044] (2) Preparation of basic electrolyte
[0045] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain a basic electrolyte;
[0046] (3) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0047] Tri-n-butylphosphonium tetrafluoroborate electrolyte additive is added to the basic electrolyte prepared in step (2), wherein the amount of the electrolyte additive is 1.5% of the mass of the basic electrolyte, to obtain a lithium-rich manganese-based lithium ion battery electrolyte.
[0048] Example 4
[0049] (1) Preparation of organic solvent for electrolyte
[0050] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0051] (2) Preparation of basic electrolyte
[0052] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain a basic electrolyte;
[0053] (3) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0054] Add tri-n-butylphosphonium tetrafluoroborate as an electrolyte additive to the basic electrolyte prepared in step (2), wherein the amount of the electrolyte additive is 2.0% of the mass of the basic electrolyte, to obtain a lithium-rich manganese-based lithium ion battery electrolyte.
[0055] Example 5
[0056] (1) Preparation of organic solvent for electrolyte
[0057] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0058] (2) Preparation of basic electrolyte
[0059] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain a basic electrolyte;
[0060] (3) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0061] Tri-n-butylphosphonium tetrafluoroborate electrolyte additive is added to the basic electrolyte prepared in step (2), wherein the amount of the electrolyte additive is 2.5% of the mass of the basic electrolyte, to obtain a lithium-rich manganese-based lithium ion battery electrolyte.
[0062] Example 6
[0063] (1) Preparation of organic solvent for electrolyte
[0064] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0065] (2) Preparation of basic electrolyte
[0066] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain a basic electrolyte;
[0067] (3) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte
[0068] The amount of tri-n-butylphosphonium tetrafluoroborate additive added to the basic electrolyte prepared in step (2) is 3.0% of the mass of the basic electrolyte to obtain a lithium-rich manganese-based lithium ion battery electrolyte.
[0069] Comparative Example 1
[0070] (1) Preparation of organic solvent for electrolyte
[0071] Cyclic carbonate solvent ethylene carbonate (EC) and linear carbonate solvent ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of EC:EMC:DEC=1:1:1, and purified by molecular sieve to remove impurities and water, thereby obtaining an electrolyte organic solvent;
[0072] (2) Preparation of electrolyte
[0073] At room temperature, dissolve the ion-conducting lithium salt LiPF6 in the organic solvent of the electrolyte in step (1) to a final concentration of 1.0 mol L -1 , stir evenly to obtain an electrolyte.
[0074] Comparison of electrochemical performance of electrolytes of Example 2 of the present invention and Comparative Example 1
[0075] The parallel test results of Li / / Pt batteries assembled with the electrolytes finally prepared in Example 2 and Comparative Example 1 are as follows: Figure 1 As shown:
[0076] Figure 1This is a comparison of the LSV curves of Li / / Pt batteries assembled using the electrolytes prepared in Comparative Example 1 and Example 2. The oxidation potential of the basic electrolyte is 4.81 V. The addition of tri-n-butylphosphonium tetrafluoroborate additive can broaden the electrochemical window to 4.83 V. After adding 1 wt.% tri-n-butylphosphonium tetrafluoroborate, the oxidation stability of the electrolyte decreases, and an increase in oxidation current begins to occur at around 3.80 V, which is mainly due to the oxidative decomposition of the tri-n-butylphosphonium tetrafluoroborate additive.
[0077] The parallel test results of lithium-rich manganese-based / / Li batteries assembled using the electrolytes finally prepared in Example 2 and Comparative Example 1 are as follows: Figure 2-Figure 4 As shown:
[0078] Figure 2 The figure is a comparison of the cycle performance of lithium-rich manganese-based / / Li batteries assembled using the electrolytes prepared in Comparative Example 1 and Example 2 at 1 C. After 340 cycles at 1 C using the basic electrolyte, the capacity retention rate is only 31.2%, while after adding 1 wt.% tri-n-butylphosphonium tetrafluoroborate additive to the basic electrolyte, the capacity retention rate of the lithium-rich manganese-based electrode reaches 79.7% after 340 cycles at a high voltage of 4.8 V, and the cycle stability is significantly improved.
[0079] Figure 3 This is a comparison diagram of electrochemical impedance of lithium-rich manganese-based / / Li batteries assembled using electrolytes prepared in Comparative Example 1 and Example 2 after cycling 200 times at 1 C. The results show that the battery using the electrolyte containing 1 wt.% tri-n-butylphosphonium tetrafluoroborate additive prepared in Example 2 has lower interfacial impedance, indicating that the decomposition of the electrolyte under high pressure is effectively suppressed.
[0080] Figure 4 The figure is a comparison of the rate performance of lithium-rich manganese-based / / Li batteries assembled with the electrolytes prepared in Comparative Example 1 and Example 2. It can be seen that the discharge specific capacity of the lithium-rich manganese-based / / Li battery at different current densities in the electrolyte with 1 wt% tri-n-butylphosphonium tetrafluoroborate added is higher than the discharge specific capacity of the lithium-rich manganese-based / / Li battery in the basic electrolyte, indicating that the rate performance of the lithium-rich manganese-based / / Li battery in the electrolyte with tri-n-butylphosphonium tetrafluoroborate added is effectively improved.
[0081] The above are only specific embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A lithium-rich manganese-based lithium-ion battery electrolyte, comprising a basic electrolyte and an electrolyte additive, wherein the basic electrolyte is a lithium salt and an electrolyte organic solvent, Its characteristics are: The electrolyte additive structural formula is: The electrolyte organic solvent is a mixed solvent of cyclic carbonate solvent ethylene carbonate and linear carbonate solvents ethyl methyl carbonate and diethyl carbonate, wherein the volume ratio of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate is 1:1:1; The electrolyte additive accounts for 0.5%-3% of the mass of the basic electrolyte.
2. The lithium-rich manganese-based lithium-ion battery electrolyte according to claim 1, Its characteristics are: The lithium salt is lithium hexafluorophosphate.
3. The lithium-rich manganese-based lithium-ion battery electrolyte according to claim 2, Its characteristics are: The concentration of lithium salt in the electrolyte is 1 mol L -1 .
4. The lithium-rich manganese-based lithium-ion battery electrolyte according to claim 1, Its characteristics are: The electrolyte additive accounts for 1% of the mass of the basic electrolyte.
5. A method for preparing the lithium-rich manganese-based lithium-ion battery electrolyte as claimed in claim 1, Its characteristics are: The steps include: (1) Preparation of basic electrolyte Ethylene carbonate, ethyl methyl carbonate and diethyl carbonate are mixed evenly, and purified by molecular sieve to remove impurities and water, and lithium salt is added to obtain a basic electrolyte; (2) Preparation of lithium-rich manganese-based lithium-ion battery electrolyte The electrolyte additive is added to the basic electrolyte to obtain a lithium-rich manganese-based lithium-ion battery electrolyte.
Citation Information
Patent Citations
Lithium ion battery electrolyte and lithium ion battery
CN107768719A
Lithium-ion battery electrolytes with improved thermal stability
US20040091772A1