A control method for dieless wheel-to-wheel flexible hot spinning

The flexible thermal spin forming control method of moldless wheels is designed by designing spinning blast material and trajectory, combined with induction heating, and solving the problems of high mold cost and low flame heating efficiency in traditional spin forming, achieving high efficiency and stable high performance. Part molding reduces production costs and risk of equipment damage.

CN117655191BActive Publication Date: 2024-11-29XIAN BOSAI SPINNING TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311712293.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-13
Publication Date
2024-11-29
Estimated Expiration
2043-12-13

AI Technical Summary

Technical Problem

Traditional forging, extrusion, rolling and welding machining processes cannot meet the high precision requirements of high-performance parts, and spin forming is limited by high mold costs and temperature unevenness of flame heating, resulting in low material utilization. , high production cost and low processing efficiency.

Method used

The flexible hot spin forming control method of moldless wheel is adopted, and the parts are efficient and uniformly heated and formed through the spinning blast material size design, spinning pass design, spinning trajectory design, spinning wheel design and induction heating device. Avoid the drawbacks of mold input and flame heating.

Benefits of technology

It reduces R&D costs, improves parts quality and processing stability, improves material utilization, reduces the risk of thermal damage of spinning equipment, and is suitable for spinning deformation of large-diameter parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117655191B_ABST
    Figure CN117655191B_ABST
Patent Text Reader

Abstract

The invention discloses a control method for moldless wheel-to-wheel flexible hot spinning, which belongs to the field of plastic processing of metal pipes. The control method for moldless wheel-to-wheel flexible hot spinning includes spinning blank size design, spinning pass design and clearance design between inner and outer wheels, spinning trajectory design, generating CNC spinning program code on programming software, spinning wheel design, measuring clearance between inner and outer wheels, determining spinning processing parameters, blank heating, preheating the blank in advance, feeding the blank into a CNC spinning machine, and providing an induction heating device at a position outside the blank in the spinning machine for spinning processing; the invention can overcome the drawbacks of die spinning, avoid mold investment, reduce research and development costs, solve the problems of uneven conventional flame heating, low production efficiency, and great control difficulty, and can improve part quality and processing stability, and induction heating can concentrate heating efficiency, which has a certain inhibitory effect on thermal damage of spinning equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of plastic processing of metal pipes, and more specifically to a dieless wheel-to-wheel flexible hot spinning forming control method. Background Art

[0002] As the aviation, aerospace, weapons, energy and other industries develop towards the direction of improving safety and reliability, the requirements for component performance and precision are getting higher and higher. Some important components use a large number of high-performance materials, and the number of high-precision rotating parts made of these materials has also increased. Most of these structural parts have complex surfaces and require very high performance and dimensional accuracy. The traditional process methods of forging, extrusion, rolling, and welding and then machining can no longer meet the high-performance requirements of the new generation of parts. Moreover, the forming thickness of the forged and extruded tubes is generally much greater than the required thickness, so a large amount of machining (generally machining methods are turning and boring) is required to meet the final requirements of the parts, and the material utilization rate is about 15-30%. This leads to large material loss and greatly increases production costs. As a result, spin forming is becoming more and more widely used.

[0003] The spinning process has many advantages in the preparation of the rotating body parts. Spinning can greatly improve processing efficiency and save raw materials. Mass production has been formed in the forming of engine casings in aerospace, weapons, etc. However, ordinary spinning processing is limited by the high cost of tooling and molds, and the complex structure of some parts makes it difficult to demold after spinning, which limits the application scope of spinning. In addition, various high-performance metal materials are often difficult to form at room temperature. Ordinary flame heating methods have disadvantages such as uneven temperature and low heating efficiency, which also restricts the spinning of moldless flexible spinning parts. In view of this, we propose a control method for moldless flexible hot spinning. Summary of the invention

[0004] The object of the present invention is to provide a dieless wheel flexible hot spinning forming control method to solve the problems raised in the above background technology:

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A dieless wheel-to-wheel flexible hot spinning forming control method comprises the following steps:

[0007] The size design of the spinning blank is to calculate the outer dimensions of the blank parts according to the required outer dimensions of the parts. The parts include A convex structure, B concave structure, C straight tube structure, and the straight tube structure is divided into equal wall thickness or variable wall thickness;

[0008] Design of spinning passes and the gap between the inner and outer spinning wheels. Calculate the part thinning rate K1 according to the required part wall thickness and blank wall thickness. Compare the part thinning rate K1 with the material single-pass limit thinning rate K0 of the wheel spinning process to calculate the thinning amount per pass and the number of spinning passes n required for part forming.

[0009] Spinning trajectory design: design the spinning trajectory according to the spinning passes;

[0010] Generate CNC spinning program code on the programming software and perform simulation test on the generated code;

[0011] Wheel design, including wheel material selection and wheel profile design;

[0012] Measure the gap between the epitrochoid and the hypotrochoid;

[0013] Determine the spinning processing parameters, including but not limited to the spinning temperature C, the spinning wheel thrust N, the rotation speed S, and the feed speed F;

[0014] Heating the blank: After preheating the blank in advance, the blank is fed into a CNC spinning machine, and an induction heating device is arranged at the outer side of the blank in the spinning machine;

[0015] Spinning processing, according to the compiled CNC spinning program, the CNC spinning machine tool communicates.

[0016] Preferably, the required part wall thickness is T1, the blank thickness is T0, and the part thinning rate K1 is calculated:

[0017]

[0018] Preferably, the comparison of the part thinning rate K1 with the material single-pass limit thinning rate K0 of the spinning process includes:

[0019] If K1≤K0, the spinning can be performed in one pass, and the thinning amount δt in one pass is determined according to the required wall thickness T1 of the part and the thickness T0 of the raw material: δt=T0-T1;

[0020] If K1>K0, multiple passes of spinning are required. The first pass thinning amount δt1 is designed according to the material's single pass limit thinning rate K0 of spinning: δt1=T0×K0;

[0021] According to the thickness T0-δt1 of the part after the first spinning pass and the required thickness T1 of the part, calculate the subsequent thinning rate K2 of the part:

[0022]

[0023] Compare K2 with K0. If K2≤K0, the part needs two passes of spinning forming. Determine the thinning amount δt2 in the second pass: δt2=T0-δt1-T1;

[0024] If K2>K0, then the second pass thinning amount δt2=δt1, and so on, calculate the subsequent thinning rate K of the part n To K n ≤K0, and the total number of spinning passes n required for part forming is obtained.

[0025] Preferably, the gap between the inner and outer wheels is calculated as follows: the gap between the inner and outer wheels at the nth pass is equal to the blank thickness T0 minus the total thinning amount from the first pass to the nth pass;

[0026] When one-pass spinning is performed, the gap between the inner and outer wheels is T0-δt;

[0027] When multiple passes of spinning are performed, the gap between the inner and outer wheels in the first pass is T0-δt1; the gap between the inner and outer wheels in the second pass is T0-δt1-δt2, and so on.

[0028] Preferably, the spinning trajectory design includes: determining whether the part is formed in one pass or multiple passes; if it is formed in multiple passes, determining the part type.

[0029] Preferably, if it is a one-step forming part, the spinning trajectory is designed according to the part profile and wall thickness changes;

[0030] If it is a multi-pass forming part, and the part type is A convex structure or B concave structure part, there is not only a change in wall thickness during the spinning process, but also a change in diameter. and minimum diameter Find the change in diameter Using the principle of equal distribution, the change in diameter direction of each pass is Design the spinning trajectory according to the diameter change and wall thickness change;

[0031] If it is a multi-pass forming part, and the part type is a C straight cylinder structure part, there is no need to consider the change in the diameter direction, and it is only necessary to design the spinning trajectory according to the change in wall thickness.

[0032] Preferably, the material of the rotating wheel should be hot working die steel with Rockwell hardness HRC ≥ 52;

[0033] The wheel profile design includes:

[0034] When the part is an A convex structure or a B concave structure part, the part surface needs to be considered when designing the wheel. The wheel surface cannot interfere with the part surface. The wheel design fillet R0 is not greater than the minimum arc angle R of the part. min ;

[0035] But if the minimum arc angle R minWhen the diameter is less than 8mm, the spinning wheel needs to be designed in two specifications, one for spinning the shape and the other for shaping the R min , shaping wheel radius R z ≤R min ;

[0036] When the part is a C straight cylinder structure part, the wheel surface is set as a single cone wheel, and the wheel surface will not interfere with the part surface.

[0037] Preferably, a standard gauge block or a feeler gauge is used to measure the gap between the inner and outer wheels, and the measurement error of the gap between the inner and outer wheels should be less than 0.05;

[0038] The blank is preheated by placing it in a resistance heating furnace for preheating before entering the spinning machine. The preheating temperature in the resistance heating furnace is not less than 300°C.

[0039] Preferably, the spinning process comprises:

[0040] An induction heating device is used to heat the billet spinning position, and the induction heating device can move axially together with the spinning wheel;

[0041] The material temperature is measured by an infrared measuring device, which can move with the induction heating device. The infrared measuring device includes a heating temperature measuring device and a molding temperature measuring device;

[0042] Spinning begins after the material temperature reaches the process requirements. The temperature is continuously measured during spinning and the measurement information is fed back to the system. The system fine-tunes the heating power according to the set temperature to ensure that the forming temperature range meets the requirements.

[0043] After each spinning pass, the thickness of the formed material is measured, and the thinning amount of the next pass is adjusted according to the thickness of the formed material.

[0044] Preferably, if the part is spun in one pass, the entire spinning process is finished;

[0045] If the part is formed by multi-pass spinning, after completing the first pass spinning thinning amount δt1, use a high-temperature thickness gauge to measure the thickness of the formed material, and adjust the second pass thinning amount δt2 appropriately according to the deviation value.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The present invention can overcome the drawbacks of die spinning, avoid mold investment, reduce R&D costs, and solve the problems of uneven conventional flame heating, low production efficiency, and difficult control, and can improve part quality and processing stability. Induction heating can concentrate heating efficiency, which has a certain inhibitory effect on thermal damage to spinning equipment. Flame heating heat is not easy to dissipate, which has a greater impact on the transmission structure and working parts. In addition, the flame heating temperature of large-diameter parts is limited, which is not conducive to the spinning deformation of parts. The dieless wheel flexible hot spinning forming control method of this application can avoid the above defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a schematic diagram of the front view of the induction heating spinning process of the present invention;

[0049] Figure 2 It is a top view schematic diagram of the induction heating spinning process of the present invention;

[0050] Figure 3 A is a schematic diagram of the convex structure part;

[0051] Figure 4 It is a schematic diagram of the concave structural parts of B;

[0052] Figure 5 It is a schematic diagram of the C straight tube structure parts.

[0053] Explanation of the numbers in the figure: 1. Blank fixing block; 2. Spinning part; 3. Induction heating device; 4. Inner rotating wheel; 5. Outer rotating wheel; 6. Heating temperature measuring device; 7. Forming temperature measuring device. DETAILED DESCRIPTION

[0054] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0055] Example:

[0056] See also Figure 1-5 , a dieless wheel flexible hot spinning forming control method, comprising the following steps:

[0057] Step 1: Design of the size of the spinning blank. According to the part structure, the dieless wheel flexible hot spinning forming parts can be roughly divided into three forming structures, such as Figure 3-5 As shown: A is an outer convex structure, B is an inner concave structure, and C is a straight tube structure. The straight tube structure is divided into equal wall thickness or variable wall thickness.

[0058] For dieless wheel flexible hot spinning, generally, the blank is obtained by machining of extruded or forged thick-walled pipe fittings. The machining allowance is generally not less than 3mm in diameter, and the inner and outer surface roughness after machining is Ra3.2.

[0059] For parts with structures A and B, the diameter of the blank The wall thickness T0 can be determined based on the required part's dimensions and wall thickness T1. The blank length L0 is calculated based on the principle that the volume remains unchanged. The volume of the required part can be calculated through 3D modeling and set as V1. The blank length calculation formula is:

[0060]

[0061] For C-structure parts, according to the required diameter of the part Wall thickness T1, length L1, (variable wall thickness requires thickness T2, length L2) to determine the diameter of the blank Wall thickness T0. Calculate the blank length L0, the calculation principle is that the volume remains unchanged (the thickness is much smaller than the diameter), the calculation formula is:

[0062] Equal wall thickness: L1×T1=L0×T0

[0063]

[0064] Variable wall thickness: L1×T1+L2×T2=L0×T0

[0065]

[0066] Step 2: Design of spinning passes and gap between inner and outer spinning wheels.

[0067] Spinning pass design. Calculate the part thinning rate K1 based on the required wall thickness T1 and raw material thickness T0 of the part:

[0068]

[0069] Compare K1 with the material's single-pass limit thinning rate K0, which is obtained through the material spinning test. If K1≤K0, one-pass spinning can be performed, and the one-pass thinning amount δt is determined based on the required wall thickness T1 of the part and the thickness T0 of the raw material: δt=T0-T1.

[0070] Determine the gap T0-δt between the hypotrochoid and the epitrochoid.

[0071] If K1>K0, multiple passes of spinning are required, and the first pass thinning amount δt1 is designed according to the material's single-pass limit thinning rate K0 of spinning: δt1=T0×K0.

[0072] Determine the gap between the inner and outer wheels in the first pass as T0-δt1. Calculate the subsequent thinning rate K2 of the part based on the thickness T0-δt1 of the part after spinning and the required thickness T1 of the part:

[0073] Compare K2 with K0. If K2≤K0, the part needs two passes of spinning forming, and the thinning amount of the second pass δt2 is determined: δt2=T0-δt1-T1.

[0074] If K2>K0, then the second pass thinning amount δt2=δt1 is designed, and the subsequent thinning rate K of the part is calculated. n To K n ≤K0, and the total number of spinning passes n required for part forming is obtained.

[0075] The gap between the inner and outer wheels is calculated as follows: the gap between the inner and outer wheels at the nth pass is equal to the blank thickness T0 minus the total thinning amount from the first pass to the nth pass;

[0076] That is, when one spinning process is performed, the gap between the inner and outer wheels is T0-δt;

[0077] When multiple passes of spinning are performed, the gap between the inner and outer wheels in the first pass is T0-δt1; the gap between the inner and outer wheels in the second pass is T0-δt1-δt2, and so on.

[0078] Step 3: Spinning trajectory design includes: determining whether the part is formed in one pass or multiple passes; determining the part type and designing the spinning trajectory according to the spinning passes.

[0079] The spinning trajectory can control the material deformation during the spinning process. If it is a one-step forming part, the spinning trajectory is designed according to the part surface and wall thickness changes.

[0080] If it is a multi-pass forming part, it needs to be distinguished according to the part structure. For parts of type A convex structure or B concave structure, there is not only a change in wall thickness during the spinning process, but also a change in diameter. According to the maximum diameter of the part and minimum diameter Find the change in diameter Using the principle of equal distribution, the change in diameter direction of each pass is Design the spinning trajectory according to the diameter change and wall thickness change. For C straight cylinder structure parts, there is no need to consider the diameter change, only the spinning trajectory needs to be designed according to the wall thickness change.

[0081] Step 4: Based on the spinning trajectory confirmed in step 3, add auxiliary lines such as feed and retract during the spinning process to ensure that the spinning wheel does not interfere with the tooling and blank during the feed and retract process, generate CNC program code on the programming software, and perform simulation detection on the generated code.

[0082] Step 5: Design of the roller. The design of the roller mainly includes the selection of roller materials and the design of roller profile. The roller material is hot working die steel with Rockwell hardness HRC ≥ 52. The design of roller profile needs to consider the part structure. When the part is an A convex structure or a B concave structure part, the part profile needs to be considered when designing the roller. The roller profile cannot interfere with the part profile. The roller design fillet R0 should generally not be greater than the minimum arc angle R of the part. min , but if the minimum arc angle R min When the diameter is less than 8mm, the spinning wheel needs to be designed in two specifications, one for spinning the shape and the other for shaping the R min , when designing the rounded corners R of the rotary wheel z ≤R min When the part is a C straight cylinder structure part, the wheel surface is set as a single cone wheel, the wheel surface will not interfere with the part surface, and the wheel fillet can be set according to the material grade and material thickness based on processing experience.

[0083] Step 6: Based on the clearance between the inner and outer wheels determined in step 2, use a standard gauge block or feeler gauge to measure the clearance between the inner and outer wheels. The measurement error of the clearance between the inner and outer wheels should be less than 0.05. The clearance between the inner and outer wheels in the first pass is T0-δt1, the clearance between the inner and outer wheels in the second pass is T0-δt1-δt2, and so on. When measuring the clearance between the inner and outer wheels, do not consider the machine tool concession, the inconsistent morphology of multiple inner and outer wheels, and do not consider the inconsistent morphology of multiple inner and outer wheels. It is assumed that the morphology of multiple inner and outer wheels is consistent.

[0084] Step 7: Set the spinning parameters. In the spinning test to determine the material spinning single pass limit thinning rate K0, the spinning parameters are confirmed through debugging, including but not limited to the spinning temperature C, spinning wheel thrust N, rotation speed S, feed speed F, etc.

[0085] Step 8: Heating the blank. Place the material to be spun in a resistance heating furnace for preheating. This step is to save the time occupied by the spinning machine and shorten the heating time of the parts on the spinning machine by preheating in advance. Preheating in the resistance heating furnace should generally not be lower than 300°C. Take out the cylindrical spinning blank preheated in the resistance furnace and use special lifting tools to quickly lift it so that the material can reduce the temperature drop. Calculate the heating power according to the size of the blank, adjust the parameters of the heating equipment in the spinning machine during the spinning process, and use an infrared thermometer to measure the heating temperature of the workpiece in real time to ensure precise temperature control during the hot spinning process. A heating device is provided at the outside of the blank in the spinning machine, and the heating device is an induction heating device.

[0086] Step 9: Spinning process: According to the CNC spinning program compiled in step 4, the CNC spinning machine tool is communicated.

[0087] Exemplarily, the heating program is started, and the spinning position of the blank is first heated by the induction heating device. During the heating process, the spindle rotates normally at a low speed, so that the uniformity of the heating temperature can be controlled. The material temperature is measured by an infrared measuring device, and spinning is started after the process requirements are met. The temperature is continuously measured during spinning and the measurement information is fed back to the system. The system fine-tunes the heating power according to the set temperature to ensure that the forming temperature range meets the requirements. Among them, the induction heating device can move axially together with the spinning wheel, and the material temperature is measured by an infrared measuring device. The infrared measuring device can move with the induction heating device. The infrared measuring device includes a heating temperature measuring device 6 and a forming temperature measuring device 7;

[0088] Through the heating device, the blank can reach the predetermined forming temperature C before the rotating wheel contacts the material, realizing high-temperature spinning of the part. In addition, the heating device moves axially together with the rotating wheel, which can keep the material in front of the rotating wheel in the process of preheating, heating and heat preservation, so that the deformation process can proceed smoothly.

[0089] After each spinning pass, the thickness of the formed material is measured, and the thinning amount of the next pass is adjusted according to the thickness of the formed material.

[0090] Step 10: If the part is spun in one pass, the entire spinning process is over. If the part is spun in multiple passes, after the first pass thinning amount δt1 is completed, a high temperature thickness gauge is used to measure the thickness of the formed material, and the second pass thinning amount δt2 is appropriately adjusted according to the deviation value. At the same time, the spinning process is carried out according to the processing flow of each pass: heating → heating spinning → measurement.

[0091] Step 11: After the entire spinning process is completed, the stripping device is used to remove the parts in a warm state, and the temperature of the parts is recorded at the same time. After cooling, the inner diameter, outer diameter, surface clearance, wall thickness, straightness, roundness and other indicators are measured.

[0092] like Figure 1-2 As shown, the spinning wheel includes an inner spinning wheel 4 and an outer spinning wheel 5. The spun part 2 is fixed on the spinning machine by a blank fixing block 1. During the spinning process, the main shaft drives the blank (i.e., the spun part 2) to rotate. Both the inner spinning wheel 4 and the outer spinning wheel 5 can rotate actively, and can also rotate passively driven by friction. The main movement mode of the spinning wheel is axial movement, which grinds and shapes the material. During operation, the heating device 3 preheats the material to be formed in front of the spinning wheel. The heating device 3 has a certain positional relationship with the spinning wheel and can move axially with the spinning wheel. In this way, the material in front of the spinning wheel can be kept preheated, heated, and kept warm, so that the deformation process can proceed smoothly. The two temperature measuring devices, namely the heating temperature measuring device 6 and the forming temperature measuring device 7, can also move with the heating device, continuously measure the temperature and feed it back to the system. The system fine-tunes the heating power according to the set temperature to ensure that the forming temperature range meets the requirements.

[0093] The present application provides a method for controlling moldless wheel-paired flexible hot spinning, which reduces the cost of the spinning core mold through moldless wheel-paired flexible spinning. In moldless wheel-paired flexible spinning, the central core mold is replaced by wheels (not limited to one pair of wheels). Only by adjusting the machine tool, pipes of any diameter within a certain range can be processed (without the need for a corresponding core mold), which can greatly reduce the cost of research and development. In addition, the constant temperature deformation of the material can be achieved by combining induction heating with moldless wheel-paired flexible spinning, which improves the stability of the spinning process and solves the problem of the adverse effects of flame heating on the quality of parts. It is applicable to moldless wheel-paired flexible hot spinning of various high-performance metal parts.

[0094] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A dieless wheel flexible hot spinning forming control method, characterized in that: The steps include: The size design of the spinning blank is to calculate the outer dimensions of the blank parts according to the required outer dimensions of the parts. The parts include A convex structure, B concave structure, C straight tube structure, and the straight tube structure is divided into equal wall thickness or variable wall thickness; For parts with A convex structure and B concave structure, the diameter of the blank The wall thickness T0 is determined according to the outer dimensions of the required part and the wall thickness T1. The blank length L0 is calculated based on the principle that the volume remains unchanged. The volume of the required part is calculated through three-dimensional modeling and is set as V1. The blank length calculation formula is: For parts with C straight structure, according to the required diameter of the parts Wall thickness T1, length L1, variable wall thickness requires thickness T2, length L2 to determine the diameter of the blank Wall thickness T0, calculate the blank length L0, the calculation principle is that the volume remains unchanged, the calculation formula is: Equal wall thickness: L1×T1=L0×T0, Variable wall thickness: L1×T1+L2×T2=L0×T0, The spinning pass design and the clearance design between the inner and outer spinning wheels are designed. According to the required part wall thickness T1 and the blank thickness T0, the part thinning rate K1 is calculated. Compare the part thinning rate K1 with the material single-pass limit thinning rate K0 of the wheel spinning, calculate the thinning amount per pass and the number of spinning passes n required for part forming; if K1≤K0, one-pass spinning can be performed, and the one-pass thinning amount δt is determined according to the required wall thickness T1 of the part and the thickness T0 of the raw material: δt=T0-T1; If K1>K0, multiple passes of spinning are required. The first pass thinning amount δt1 is designed according to the material's single pass limit thinning rate K0 of spinning: δt1=T0×K0; According to the thickness T0-δt1 of the part after the first spinning pass and the required thickness T1 of the part, calculate the subsequent thinning rate K2 of the part: Compare K2 with K0. If K2≤K0, the part needs two passes of spinning forming. Determine the thinning amount δt2 in the second pass: δt2=T0-δt1-T1; If K2>K0, then the second pass thinning amount δt2=δt1, and so on, calculate the subsequent thinning rate K of the part n To K n ≤K0, the total number of spinning passes n required for part forming is obtained; The gap between the inner and outer wheels is calculated as follows: the gap between the inner and outer wheels at the nth pass is equal to the blank thickness T0 minus the total thinning amount from the first pass to the nth pass; That is, when one spinning process is performed, the gap between the inner and outer wheels is T0-δt; When multiple passes of spinning are performed, the gap between the inner and outer wheels in the first pass is T0-δt1; the gap between the inner and outer wheels in the second pass is T0-δt1-δt2, and so on; Spinning trajectory design: design the spinning trajectory according to the spinning passes: determine whether the part is formed in one pass or multiple passes; if it is formed in multiple passes, determine the part type; If it is a one-step forming part, the spinning trajectory is designed according to the part profile and wall thickness changes; If it is a multi-pass forming part, and the part type is A convex structure or B concave structure part, there is not only a change in wall thickness during the spinning process, but also a change in diameter. and minimum diameter Find the change in diameter Using the principle of equal distribution, the change in diameter direction of each pass is Design the spinning trajectory according to the diameter change and wall thickness change; If it is a multi-pass forming part, and the part type is a C straight cylinder structure part, there is no need to consider the change in the diameter direction, and only the spinning trajectory needs to be designed according to the change in wall thickness; Generate CNC spinning program code on the programming software and perform simulation test on the generated code; Wheel design, including wheel material selection and wheel profile design; The material of the rotating wheel is hot working die steel, Rockwell hardness HRC ≥ 52; The wheel profile design includes: when the part is an A convex structure or a B concave structure part, the wheel profile needs to be considered when designing the wheel, the wheel profile cannot interfere with the part profile, and the wheel design fillet R0 is not greater than the minimum arc angle R min ; But if the minimum arc angle R min When the diameter is less than 8mm, the spinning wheel needs to be designed in two specifications, one for spinning the shape and the other for shaping the R min , shaping wheel radius R z ≤R min ; When the part is a C straight cylinder structure part, the wheel surface is set as a single cone wheel, and the wheel surface will not interfere with the part surface; Measure the gap between the epitrochoid and the hypotrochoid; Determine the spinning processing parameters, including but not limited to the spinning temperature C, the spinning wheel thrust N, the rotation speed S, and the feed speed F; Heating the blank: After preheating the blank in advance, the blank is fed into a CNC spinning machine, and an induction heating device is arranged outside the blank in the spinning machine; Spinning processing, according to the compiled CNC spinning program, the CNC spinning machine tool communicates.

2. A dieless wheel pair flexible hot spinning forming control method according to claim 1, characterized in that: Use a standard gauge block or feeler gauge to measure the gap between the inner and outer wheels. The measurement error of the gap between the inner and outer wheels should be less than 0.

05. The blank is preheated by placing it in a resistance heating furnace for preheating before entering the spinning machine. The preheating temperature in the resistance heating furnace is not less than 300°C.

3. A dieless wheel pair flexible hot spinning forming control method according to claim 1, characterized in that: The spinning process comprises: An induction heating device is used to heat the billet spinning position, and the induction heating device can move axially together with the spinning wheel; The material temperature is measured by an infrared measuring device, which can move with the induction heating device. The infrared measuring device includes a heating temperature measuring device and a molding temperature measuring device; Spinning begins after the material temperature reaches the process requirements. The temperature is continuously measured during spinning and the measurement information is fed back to the system. The system fine-tunes the heating power according to the set temperature to ensure that the forming temperature range meets the requirements. After each spinning pass, the thickness of the formed material is measured, and the thinning amount of the next pass is adjusted according to the thickness of the formed material.

4. A dieless wheel pair flexible hot spinning forming control method according to claim 3, characterized in that: If the part is spun in one pass, the entire spinning process is complete; If the part is formed by multi-pass spinning, after completing the first pass spinning thinning amount δt1, use a high-temperature thickness gauge to measure the thickness of the formed material, and adjust the second pass thinning amount δt2 appropriately according to the deviation value.

Citation Information

Patent Citations

  • Coreless spinning machining method for large-scale multi-variable-diameter hollow shaft

    CN110548797A

  • Six-wheel powerful staggered spinning forming method for large-diameter pure titanium cylindrical part

    CN116274371A