Anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane and its preparation method and application
By grafting the perfluorosulfonic acid fluorine resin with anion cationic radiation graft modification, the problem of difficult to take into account both the conductivity and the permeability of vanadium battery film materials in the existing vanadium battery film materials, and high-performance amphoteric perfluorosulfonic acid ions were prepared. The exchange membrane improves the separator performance of vanadium batteries.
Patent Information
- Application Number
- CN202311662315.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-12-06
AI Technical Summary
The existing vanadium battery film materials are difficult to reduce the permeability of vanadium ions while increasing the conductivity, resulting in the limitation of the use performance of vanadium batteries.
By grafting the perfluorosulfonic acid fluorine resin with anion grafting modification, branching structure is increased, and combined with gamma ray irradiation technology, a uniformly distributed grafted anion and cation exchange membrane is prepared to reduce the permeability of vanadium ions. and improve conductivity.
An amphoteric perfluorosulfonic acid ion exchange membrane with uniform thickness and smooth surface is achieved, which significantly reduces the permeability of vanadium ions and improves the comprehensive use performance of vanadium battery separators.
Abstract
Description
Technical Field
[0001] The invention relates to an anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane and a preparation method and application thereof, belonging to the field of vanadium battery ion exchange membranes. Background Art
[0002] Compared with other energy storage batteries, vanadium redox flow batteries (VRBs) have the characteristics of high energy efficiency, short response time, low self-discharge rate, and long cycle life, and therefore have attracted widespread attention and application. Vanadium redox flow batteries are considered to be a highly efficient energy storage / conversion system. Their design capacity is much larger than that of conventional batteries, and they have obvious advantages. They can be connected to the power system on a large scale and are widely used in large-scale energy storage devices such as load balancing, grid peak regulation, and uninterruptible power supplies (UPS).
[0003] At present, as one of the key components of redox flow batteries, membrane materials are used to separate positive and negative half-cells, and also need to provide channels for charge-balancing ions to ensure the battery circuit. In recent years, basic research and industrial application research on membrane materials for vanadium batteries have received widespread attention and have made great progress. According to different mechanisms, membrane materials for vanadium batteries can be divided into cation exchange membranes (CEM), anion exchange membranes (AEMS), amphoteric ion exchange membranes (ALEM) and porous membranes. The resin material of Nafion membrane is sulfonated tetrafluoroethylene polymer, which has high conductivity and is the most widely used cation exchange membrane material, but the vanadium permeability is large; while the anion exchange membrane reduces the permeation of vanadium ions due to the Donnan exclusion effect, but is also limited by low conductivity; therefore, the research direction in this field is to prepare amphoteric ion exchange membranes with both high conductivity and low vanadium ion permeability in a method suitable for mass production. Summary of the invention
[0004] In view of the problems existing in the background technology, the purpose of the present invention is to provide an anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane and a preparation method thereof. By efficiently and uniformly performing anion and cation irradiation grafting modification on perfluorosulfonic acid fluorine resin, on the one hand, a higher proportion of branched structure is given to the perfluorosulfonic acid fluorine resin, so that the resin has lower crystallinity, and the proportion of amorphous is increased, so that the resin has stable fluidity and viscoelasticity within the processing temperature range, and is easier to process and shape. An amphoteric perfluorosulfonic acid ion exchange membrane with uniform thickness and smooth surface is successfully prepared by an extrusion casting method; on the other hand, the anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane prepared by the method has uniformly distributed grafted anions and cations on the whole, not only the anions maintain a good conductivity of the film, but also the Donnan exclusion effect of the cations reduces the penetration of vanadium ions, improves the barrier property of vanadium ions, and greatly improves the comprehensive performance of the vanadium battery separator.
[0005] In order to achieve the above-mentioned object, the present invention provides a preparation method of anion-cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane, comprising the following steps: (1) fully mixing raw materials including perfluorosulfonic acid fluorine-type resin powder, anion modifier, cation modifier and grafting aid in a high-speed mixer in proportion, drying to obtain a mixed powder, drying the mixed powder and placing it in a reaction kettle, heating to 95-100° C., exhausting gas and filling with inert gas, and then sealing, irradiating with gamma rays, with an irradiation dose of 2.5-3 Mrad, and cooling to room temperature to obtain a grafted mixed powder; (2) treating the grafted mixed powder described in step (1) with an exhaust gas; The method comprises the following steps: extruding and granulating the masterbatch by a pneumatic twin-screw extruder, cooling and drying the masterbatch to obtain a masterbatch; (3) heating the masterbatch in step (2) to 95-100° C. again, subjecting the masterbatch to secondary gamma ray irradiation with an irradiation dose of 2.5-3.5 Mrad, and cooling the masterbatch to room temperature to obtain an irradiated grafted masterbatch; (4) placing the irradiated grafted masterbatch in step (3) into a single-screw extruder, melt-extruding and casting the masterbatch to film formation, and cooling the masterbatch to obtain an anion and cation irradiated grafted modified perfluorosulfonic acid resin membrane; and (5) subjecting the anion and cation irradiated grafted modified perfluorosulfonic acid resin membrane in step (4) to sodiumization and hydrogenation in sequence to obtain anion and cation irradiated grafted modified perfluorosulfonic acid ion exchange membrane.
[0006] Optionally, the anion modifier is one or a combination of styrene sulfonic acid, sodium styrene sulfonate and 3-sulfonyl methacrylate.
[0007] Optionally, the cationic modifier is one or a combination of dimethylaminoethyl methacrylate, N-(4-vinylbenzyl)-N,N-dialkylamine, N-isopropylacrylamide, methacryloyloxyethyltrimethylammonium chloride and 1-allyl-3-vinylimidazole acetate.
[0008] Optionally, the grafting aid is p-fluorostyrene.
[0009] Optionally, the raw material also includes a solvent; the solvent is ethylene dichloride or toluene.
[0010] Optionally, the mass ratio of perfluorosulfonic acid fluorine-type resin powder, anion modifier, cationic modifier, grafting aid and solvent is 100:(3-5):(5-8):(0.8-1.2):(10-20).
[0011] Optionally, the drying temperature of step (1) is 90-100° C.; the number of times of exhausting the gas and filling with the inert gas is 3-5 times; and the inert gas is nitrogen or argon.
[0012] Optionally, the venting twin-screw extruder of step (2) and the single-screw extruder of step (3) have screws, barrels and die heads made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the venting twin-screw extruder is 275-295°C, and the head temperature is 280-285°C; the temperature of each section of the single-screw extruder is 270-295°C, and the head temperature is 286-290°C.
[0013] Optionally, the sodiumization and hydrogenation in step (5) are specifically to sodiumize the anion and cation irradiation grafted modified perfluorosulfonic acid resin membrane in step (4) with a 25wt% NaOH methanol solution and hydrogenate it with a 16wt% hydrochloric acid solution, wash it with deionized water, and dry it to obtain anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane.
[0014] The present invention also provides an anion and cation radiation grafted modified perfluorosulfonic acid ion exchange membrane prepared by the method described above.
[0015] The present invention also provides an application of the above-mentioned anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane, wherein the anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane is used in vanadium batteries.
[0016] The beneficial effects of the present invention are as follows:
[0017] 1. In the present application, an anion modifier, a cationic modifier and a grafting aid are evenly distributed on the surface of the powder by a solvent, and then the solvent is removed by drying. Then, the resin is activated by gamma ray irradiation under the protection of an inert gas. The grafting aid plays an auxiliary role in grafting specific anion and cation modifiers onto the activated perfluorosulfonic acid fluorine resin, thereby increasing the branching degree of the perfluorosulfonic acid fluorine resin, maintaining stable fluidity during processing, weakening the shear-thinning non-Newtonian fluid properties, and having suitable viscoelasticity, which is convenient for extrusion casting processing to prepare amphoteric perfluorosulfonic acid ion exchange membranes.
[0018] 2. The method of the present invention can obtain an amphoteric perfluorosulfonic acid resin membrane with uniform film thickness and smooth surface. The amphoteric ion exchange membrane significantly reduces the permeability of vanadium ions while maintaining good electrical conductivity. DETAILED DESCRIPTION
[0019] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.
[0020] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0021] Raw materials: Perfluorosulfonic acid fluorine resin powder, DuPont; other raw materials, commercially available.
[0022] Example 1
[0023] (1) fully mixing raw materials of perfluorosulfonic acid fluorine resin powder, sodium styrene sulfonate, dimethylaminoethyl methacrylate, p-fluorostyrene and dichloroethane in a high-speed mixer according to a proportion, drying at 90° C. to obtain a mixed powder, drying the mixed powder and placing it in a reaction kettle, heating it to 95° C., exhausting the gas and filling it with nitrogen or argon three times, then sealing it, irradiating it with gamma rays, the irradiation dose is 2.5 Mrad, cooling it to room temperature, and obtaining a grafted mixed powder; the mass ratio of perfluorosulfonic acid fluorine resin powder, sodium styrene sulfonate, dimethylaminoethyl methacrylate, p-fluorostyrene and dichloroethane is 100:3:5:0.8:10;
[0024] (2) extruding the grafted mixed powder described in step (1) into granules by a vented twin-screw extruder, cooling, and drying to obtain master batches; the vented twin-screw extruder has a screw, a barrel, and a die head made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the vented twin-screw extruder is 290-295° C., and the die head temperature is 285° C.;
[0025] (3) heating the masterbatch in step (2) to 95° C. again, irradiating it with gamma rays for the second time at a dose of 2.5 Mrad, and cooling it to room temperature to obtain an irradiated graft masterbatch;
[0026] (4) putting the irradiated grafting masterbatch of step (3) into a single screw extruder, melting and extruding it to form a film, and cooling it to obtain an anionic and cationic irradiated grafted modified perfluorosulfonic acid resin film; the single screw extruder has a screw, a barrel and a die head made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the single screw extruder is 290-295° C., and the head temperature is 290° C.;
[0027] (5) The anion and cation irradiation grafted modified perfluorosulfonic acid resin membrane described in step (4) was sequentially sodiumized with a 25wt% NaOH methanol solution and hydrogenated with a 16wt% hydrochloric acid solution, washed with deionized water, and dried to obtain anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane.
[0028] Example 2
[0029] (1) fully mixing a perfluorosulfonic acid fluorine resin powder, 3-sulfonic acid propyl methacrylate, N-isopropylacrylamide, p-fluorostyrene and toluene in a high-speed mixer according to a certain proportion, drying at 100° C. to obtain a mixed powder, drying the mixed powder and placing it in a reaction kettle, heating it to 100° C., excluding the gas and filling it with nitrogen or argon for 5 times, and then sealing it, irradiating it with gamma rays, with an irradiation dose of 3 Mrad, and cooling it to room temperature to obtain a grafted mixed powder; the mass ratio of the perfluorosulfonic acid fluorine resin powder, 3-sulfonic acid propyl methacrylate, N-isopropylacrylamide, p-fluorostyrene and toluene is 100:5:8:1.2:20;
[0030] (2) extruding the grafted mixed powder described in step (1) into granules by using a vented twin-screw extruder, cooling, and drying to obtain master batches; the vented twin-screw extruder has a screw, a barrel, and a die head made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the vented twin-screw extruder is 275-285° C., and the die head temperature is 280° C.;
[0031] (3) heating the masterbatch in step (2) to 100° C. again, irradiating it with gamma rays for the second time at a dose of 3.5 Mrad, and cooling it to room temperature to obtain an irradiated grafted masterbatch;
[0032] (4) putting the irradiated grafted masterbatch of step (3) into a single screw extruder, melting and extruding it, and blowing it into a film through a film blowing die, and after cooling, obtaining an anionic and cationic irradiated grafted modified perfluorosulfonic acid resin film; the single screw extruder has a screw, a barrel and a die head made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the single screw extruder is 270-288° C., and the head temperature is 286° C.;
[0033] (5) The anion and cation irradiation grafted modified perfluorosulfonic acid resin membrane described in step (4) was sequentially sodiumized with a 25wt% NaOH methanol solution and hydrogenated with a 16wt% hydrochloric acid solution, washed with deionized water, and dried to obtain anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane.
[0034] Example 3
[0035] (1) fully mixing a perfluorosulfonic acid fluorine resin powder, 3-sulfonic acid propyl methacrylate, 1-allyl-3-vinylimidazole acetate, p-fluorostyrene and ethylene dichloride in a high-speed mixer according to a certain proportion, drying at 95° C. to obtain a mixed powder, drying the mixed powder and placing it in a reaction kettle, heating it to 98° C., venting the gas and filling it with nitrogen or argon for 4 times, then sealing it, irradiating it with gamma rays, with an irradiation dose of 2.8 Mrad, and cooling it to room temperature to obtain a grafted mixed powder; the mass ratio of the perfluorosulfonic acid fluorine resin powder, 3-sulfonic acid propyl methacrylate, 1-allyl-3-vinylimidazole acetate, p-fluorostyrene and ethylene dichloride is 100:4:6.5:1:15;
[0036] (2) extruding the grafted mixed powder described in step (1) into granules by using a vented twin-screw extruder, cooling, and drying to obtain master batches; the vented twin-screw extruder has a screw, a barrel, and a die head made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the vented twin-screw extruder is 280-290° C., and the die head temperature is 283° C.;
[0037] (3) heating the masterbatch in step (2) to 98° C. again, irradiating it with gamma rays for the second time at an irradiation dose of 2.8 Mrad, and cooling it to room temperature to obtain an irradiated grafted masterbatch;
[0038] (4) putting the irradiated grafted masterbatch of step (3) into a single screw extruder, melting and extruding, and blowing into a film through a film blowing die, and cooling to obtain an anionic and cationic irradiated grafted modified perfluorosulfonic acid resin film; the single screw extruder has a screw, a barrel and a die head made of corrosion-resistant nickel-based alloy steel; the temperature of each section of the single screw extruder is 285-290° C., and the head temperature is 288° C.;
[0039] (5) The anion and cation irradiation grafted modified perfluorosulfonic acid resin membrane described in step (4) was sequentially sodiumized with a 25wt% NaOH methanol solution and hydrogenated with a 16wt% hydrochloric acid solution, washed with deionized water, and dried to obtain anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane.
[0040] Comparative Example 1
[0041] Except that p-fluorostyrene is not added, the other steps are the same as those in Example 3.
[0042] Performance Testing
[0043] The properties of the resins and films of the embodiments and comparative examples were tested respectively, and the specific test data are shown in Table 1 below.
[0044] Table 1
[0045] Test items Example 1 Example 2 Example 3 Comparative Example 1 Appearance Smooth surface Smooth surface Smooth surface Slightly rough surface Thickness / um 20±0.6 20±0.6 20±0.6 23±1 Conductivity at 25℃ / mS / cm 102.0 102.5 101.8 100.5 <![CDATA[Vanadium ion permeability / cm -2 / cm]]> <![CDATA[0.75×10 -7 ]]> <![CDATA[0.82×10 -7 ]]> <![CDATA[0.71×10 -7 ]]> <![CDATA[1.3×10 -7 ]]>
[0046] It can be seen from the data of the embodiments and comparative examples that the present invention uses para-fluorostyrene to assist the perfluorosulfonic acid fluorine resin in the irradiation grafting modification of anions and cations, so that the grafting rate of the perfluorosulfonic acid fluorine resin is greatly improved. The branched structure further improves the viscoelasticity of the resin while maintaining the flow rate and thermal stability, and improves the processability. The film product obtained by extrusion casting is flat and smooth, with a thinner and more uniform thickness and good dimensional stability. The conductivity retention rate of the perfluorosulfonic acid ion exchange membrane after sodium and acid treatment is high, and the vanadium ion isolation effect is significantly improved, which meets the comprehensive performance requirements for actual use.
[0047] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for preparing anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane, characterized in that: The following steps are involved: (1) mixing raw materials including perfluorosulfonic acid fluorine resin powder, anion modifier, cationic modifier, grafting aid and solvent in a high-speed mixer in proportion, drying to obtain a mixed powder, drying the mixed powder and placing it in a reaction kettle, heating it to 95-100° C., removing gas and filling it with inert gas, then sealing it, irradiating it with gamma rays, the irradiation dose is 2.5-3 Mrad, cooling it to room temperature, and obtaining a grafted mixed powder, wherein the mass ratio of perfluorosulfonic acid fluorine resin powder, anion modifier, cationic modifier, grafting aid and solvent is 100:(3-5):(5-8):(0.8-1.2):(10-20); (2) extruding the grafted mixed powder described in step (1) into granules using a vented twin-screw extruder, cooling, and drying to obtain master batches; (3) heating the masterbatch in step (2) to 95-100° C. again, irradiating it with gamma rays for a second time at a irradiation dose of 2.5-3.5 Mrad, and cooling it to room temperature to obtain an irradiated grafted masterbatch; (4) putting the irradiated grafted masterbatch of step (3) into a single screw extruder, melting and extruding it to form a film, and cooling it to obtain an anionic and cationic irradiated grafted modified perfluorosulfonic acid resin film; (5) subjecting the anion and cation irradiation grafted modified perfluorosulfonic acid resin membrane described in step (4) to sodiumization and hydrogenation in sequence to obtain anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane; The anion modifier is one or a combination of two or more of styrene sulfonic acid, sodium styrene sulfonate and 3-sulfonyl methacrylate; The cationic modifier is one or a combination of two or more of dimethylaminoethyl methacrylate, N-(4-vinylbenzyl)-N,N-dialkylamine, N-isopropylacrylamide, methacryloyloxyethyltrimethylammonium chloride and 1-allyl-3-vinylimidazole acetate; The grafting auxiliary agent is p-fluorostyrene; The solvent is ethylene dichloride or toluene.
2. The method for preparing the anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane according to claim 1, characterized in that: The drying temperature of step (1) is 90-100° C.; the number of times of exhausting gas and filling with inert gas is 3-5 times; and the inert gas is nitrogen or argon.
3. The method for preparing the anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane according to claim 1, characterized in that: The sodiumization and hydrogenation of step (5) are specifically to sodiumize the anion and cation irradiation grafted modified perfluorosulfonic acid resin membrane of step (4) with a 25wt% NaOH methanol solution and hydrogenate it with a 16wt% hydrochloric acid solution, wash it with deionized water, and dry it to obtain anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane.
4. An anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane prepared by the method according to any one of claims 1 to 3.
5. The use of the anion and cation irradiation grafted modified perfluorosulfonic acid ion exchange membrane as claimed in claim 4, characterized in that: The anion and cation radiation grafted modified perfluorosulfonic acid ion exchange membrane is used in vanadium batteries.
Citation Information
Patent Citations
Preparation method of amphoteric ion exchange membrane
CN102181069A
Preparation method of quaternized amphoteric ion exchange membrane
CN103242552A
Zwitter Nafion ion exchange membrane for vanadium batteries and preparation method thereof
CN108695534A
Improved method for preparing perfluorosulfonic acid ion exchange membrane through melt extrusion blow molding, thin film prepared through method and application of thin film
CN117162553A
Amphoteric electrolyte membrane with selective and balanced ion transport properties and a redox flow battery comprising an electrolyte membrane
US20210210770A1
Cited By
Material surface high-precision directional irradiation grafting method based on synchrotron radiation
CN119560209A
A high-precision directional irradiation grafting method for material surfaces based on synchrotron radiation