Composite material molded product and preparation method and system thereof
By mixing waste wind power blades with wood chips and modified MDI glue molded products, the problem of recycling and processing of wind power blades after decommissioning is solved, the goal of resource utilization and environmental protection is achieved, and efficient and environmentally friendly solutions are provided, which reduces processing costs and reduces the cost of treatment. Pollution.
Patent Information
- Application Number
- CN202311693656.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-12-11
AI Technical Summary
After the wind power blades are retired, the matrix material is epoxy resin and glass fiber, which cannot be used again, resulting in difficulty in recycling and processing and high pollution and storage costs. The existing treatment methods such as open-pit stacking, landfill and incineration have pollution problems, which affects the ecological environment. .
Use waste wind power blades, wood chips and modified MDI glue to mix molded products, and use composite molded products to regulate material proportions and process parameters to prepare composite molded products for production of pallets, building formwork and other products to achieve resource application and environmental protection goals.
It has achieved environmentally friendly and energy-saving utilization of waste wind power blades, reduced treatment costs, and the product has high load-bearing capacity, stability and environmentally friendly properties, meets the requirements of green development, and does not generate wastewater, waste gas, or waste slag, and supports the development of the new energy industry chain.
Smart Images

Figure CN117700934B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite material molded product and a preparation method and system thereof, belonging to the field of molded products and the technical field of solid waste treatment. Background Art
[0002] As one of the renewable energy sources, wind power has always been labeled as "clean" and "environmentally friendly". As a green energy source, the life of wind turbines is generally 20 to 25 years. The first generation of wind turbines began to be launched on a large scale in the 1990s. Today, many wind turbine blades have reached the end of their lives. The problem of achieving green and harmless treatment of the entire life cycle, green treatment of retired blades, and environmentally friendly reuse of retired blades has gradually been put on the table with the development of the wind power industry.
[0003] At present, the matrix materials used for wind turbine blades are epoxy resin and glass fiber, which cannot be reused after solidification, increasing the difficulty of subsequent recycling and reuse; and the glass fiber is solidified in the fiber body, making it extremely difficult to recycle. Even if it is recycled, it faces the problems of pollution and high storage costs.
[0004] At present, most of the waste blades are disposed of in open-air piles, landfills and incineration, which cause dust, emissions and many other pollution problems, seriously affecting the ecological environment. As the size and number of wind turbine blades continue to increase, the impact of these blades on the environment after retirement cannot be ignored.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a composite molded product and a preparation method and system thereof, which uses retired wind turbine blades as raw materials to produce composite molded products and other products, thereby realizing the resource application of retired wind turbine blade composite materials, while protecting the environment, saving energy and reducing emissions.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] In a first aspect, a composite molded product is provided. The composite molded product is obtained by mixing waste wind turbine blades, wood chips and modified MDI glue and then molding them. The matrix material of the waste wind turbine blades is epoxy resin and glass fiber.
[0009] Furthermore, the weight ratio of the waste wind turbine blades, wood chips and modified MDI glue is (0.5-0.9): (0.05-0.45): (0.03-0.05), and the total of the three is 1.
[0010] Furthermore, the total moisture content of the waste wind turbine blades and wood chips is 10-15%;
[0011] And / or, the modified MDI glue comprises, by mass fraction, 26-49% of diphenylmethane diisocyanate, 50-64% of polymethylene polyphenyl polyisocyanate and 1-10% of urethane modified isocyanate.
[0012] Furthermore, the waste wind turbine blades are mixed with sawdust and modified MDI glue in the form of particles and then molded, and the particle size of the waste wind turbine blades is 10-20 mm;
[0013] And / or, the particle size of the wood chips is 10-20 mm.
[0014] Further, the molding temperature is 135-155°C, preferably 150°C;
[0015] And / or, the curing time of the molding is 180 to 300 seconds, preferably 180 seconds;
[0016] And / or, the molding pressure is 15-20MPa;
[0017] And / or, the composite molded product is one or more of a molded pallet, a building formwork, a cable drum, a simple board house, a fence, a highway guardrail, and an urban municipal environmental protection manhole cover.
[0018] In a second aspect, a method for preparing the composite molded product is provided, the method comprising the following steps:
[0019] S1. Shredding the waste wind turbine blades into coarse powder and crushing them into fine powder to obtain waste wind turbine blade particles;
[0020] S2. Mixing the waste wind turbine blade particles with wood chips and modified MDI glue and then performing molding to obtain the composite molded product.
[0021] Furthermore, in step S1, the thickness of the waste wind turbine blades is not greater than 8 cm; and / or the particle size of the waste wind turbine blade particles is 10-20 mm.
[0022] Further, in step S2, the particle size of the sawdust is 10-20 mm;
[0023] And / or, the modified MDI glue comprises, by mass fraction, 26-49% of diphenylmethane diisocyanate, 50-64% of polymethylene polyphenyl polyisocyanate and 1-10% of urethane modified isocyanate;
[0024] And / or, when mixed, the total moisture content of the waste wind turbine blade particles and wood chips is 10-15%; further, when the total moisture content is lower than 10%, water is added during mixing to make the total moisture content at least 10%; when the total moisture content is higher than 15%, the total moisture content is reduced to at most 15% by drying before mixing;
[0025] And / or, the weight ratio of the waste wind turbine blade particles, wood chips and modified MDI glue is (0.5-0.9): (0.05-0.45): (0.03-0.05), and the total of the three is 1.
[0026] In a third aspect, a system for preparing the aforementioned composite molded products is provided, the preparation system comprising a feeding conveyor, a shredder, a crusher, a dryer, a storage bin, a glue mixer and a molding machine connected in sequence along the material output direction; wherein the storage bin comprises a blade storage bin and a wood chip storage bin.
[0027] Furthermore, the shredder, pulverizer, dryer and storage bin are all provided with dust removal devices;
[0028] And / or, the dryer and the molding machine are further connected via a mold temperature controller;
[0029] And / or, a buffer silo is provided between the shredder and the pulverizer;
[0030] And / or, the dryer is a rotor dryer.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The composite material molded product of the present invention is mainly made of waste wind turbine blades and waste wood chips. The product is environmentally friendly and energy-saving, and its various indicators are far higher than those of similar products, and its cost is lower than that of similar products. It not only meets the requirements for harmless treatment of retired wind turbine blades, but also meets market requirements.
[0033] 2. The composite molded pallet of the present invention is 1.2m long, 1m wide, 15cm high and 22kg in weight. In terms of load-bearing capacity, the dynamic load is ≥2.7 tons and the static load is 10-15 tons. In terms of stability, the shape is stable and does not twist. It can be used on one side and has four-way fork access. The strength and rigidity are constant. In terms of transportation efficiency, a 40-foot high cabinet can load 1,650 sheets. In terms of environmental protection attributes, it can be recycled and repeatedly produced.
[0034] 3. The preparation method and system of the composite molded products of the present invention are developed and designed based on the inherent material properties of wind turbine blades. The process is mature and the equipment is reliable. No wastewater, waste gas, or waste residue is generated during the recycling and production process of waste wind turbine blades, which is in line with the development of recyclable, green, clean, and pollution-free. On the one hand, it can serve the effective complementary advantages of the upstream industry of new energy, the downstream recycling industry, and the related industrial chain. On the other hand, it can make full use of the advantages of new energy resources and drive the development of subsequent supporting facilities for new energy power generation. Using the preparation method or system of the present invention, molded products such as molded pallets, municipal construction materials (building templates, cable reels, simple board houses, fences, etc.), high-speed guardrails, and urban municipal environmental protection manhole covers can be produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The process flow chart of the composite material molded product of the present invention;
[0036] Figure 2 It is a schematic diagram of the front and back structures of the composite material molded pallet of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0039] In the present invention, unless otherwise specified and / or described, all numerical values involving the amount of components are "weight ratios" from beginning to end. The process parameters in the following examples that do not specify specific conditions are usually based on conventional conditions. The raw materials described in the following examples can all be obtained from public commercial channels.
[0040] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0041] According to a first aspect of the present invention, a composite molded product is provided. The composite molded product is obtained by mixing waste wind turbine blades, wood chips and modified MDI glue and then molding them. The matrix material of the waste wind turbine blades is epoxy resin and glass fiber.
[0042] The composite molded product of the present invention is a molded product produced mainly by using relatively difficult-to-process solid waste materials (waste wind turbine blades). The matrix materials that account for the main components of the waste wind turbine blades are epoxy resin and glass fiber, and also contain a small amount of other components such as balsa wood. In order to ensure its use characteristics, wood chip materials must be added during the production process to improve the load-bearing capacity and surface finish. The wood chip materials can be recycled waste wood chip materials or other wood chip materials, preferably waste materials, and their waste problem is solved by recycling and reuse. The glue added in the production is: modified MDI glue, which includes 26-49% diphenylmethane diisocyanate, 50-64% polymethylene polyphenyl polyisocyanate and 1-10% urethane modified isocyanate by mass fraction. This glue and an appropriate amount of water react at high temperature to form a thermosetting cross-linked network structure, which has the effects of surface film formation, hydroxyl muscle formation, and fiber bone formation. The molded product of the present invention uses waste wind turbine blades and wood chips as raw materials, which are mixed with modified MDI glue. The modified MDI glue reacts with moisture in raw materials such as wood chips at high temperature to form a polyurea cross-linked structure. The polymer polymerization method makes the internal meridians of the molded product deep, dense and without gaps, thereby achieving performance improvement.
[0043] The composite molded product of the present invention can be a molded pallet, and can be used as a green new material pallet, which not only expands the use scenarios and application scope of the pallet and promotes green innovation in the pallet industry, but also can recycle waste wind turbine blades and waste wood chips as raw materials, improve the recycling rate of resources and waste, make a contribution to environmental protection, and effectively achieve sustainable green development.
[0044] The composite molded pallet of the present invention has a load-bearing capacity of ≥2.7 tons for dynamic load and 10-15 tons for static load. In terms of stability, it has a stable shape without distortion, can be used on one side and has four-way fork access, and has constant strength and rigidity. In terms of transportation efficiency, a 40-foot high cabinet can load 1,650 sheets. In terms of environmental protection properties, it can be recycled and repeatedly produced.
[0045] In addition, the present invention uses waste wind turbine blades + wood chips + modified MDI glue to mold and produce pallets, which can also be used to prepare and produce other molded products, such as building templates, cable reels, simple board houses, fences, etc. for municipal construction materials. It can also be used for related environmentally friendly products such as highway guardrails, urban municipal environmentally friendly manhole covers, etc., thereby achieving the purpose of environmental protection and recycling.
[0046] As an optional embodiment of the product of the present invention, the weight ratio of the waste wind turbine blades, wood chips and modified MDI glue is (0.5-0.9): (0.05-0.45): (0.03-0.05), and the total of the three is 1.
[0047] In the above technical solution, by adjusting the weight ratio within the range, such as 0.5:0.45:0.05, 0.6:0.35:0.05, 0.7:0.26:0.04, 0.8:0.16:0.04, 0.9:0.07:0.03, etc., the obtained molded product has high strength and a smooth surface.
[0048] As an optional embodiment of the product of the present invention, the total moisture content of the waste wind turbine blades and wood chips is 10-15% (such as 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, etc.).
[0049] As an optional embodiment of the product of the present invention, the waste wind turbine blades are mixed with sawdust and modified MDI glue in the form of particles and then molded, and the particle size of the waste wind turbine blades is 10-20 mm (such as 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, etc.);
[0050] And / or, the particle size of the wood chips is 10-20 mm (such as 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, etc.).
[0051] As an optional embodiment of the product of the present invention, the molding temperature is 135-155°C (such as 136°C, 138°C, 140°C, 142°C, 144°C, 146°C, 148°C, 150°C, 152°C, 154°C, etc.), preferably 150°C;
[0052] And / or, the curing time of the molding is 180 to 300 seconds (such as 190 seconds, 210 seconds, 230 seconds, 250 seconds, 270 seconds, 290 seconds, etc.), preferably 180 seconds;
[0053] And / or, the molding pressure is 15-20 MPa (such as 15.5 MPa, 16 MPa, 16.5 MPa, 17 MPa, 17.5 MPa, 18 MPa, 18.5 MPa, 19 MPa, 19.5 MPa, etc.).
[0054] In the above technical solution, the molding time, temperature and pressure are controlled within the above ranges, so that products with high output and good quality can be obtained.
[0055] According to a second aspect of the present invention, a method for preparing a composite molded product comprises the following steps:
[0056] S1. Shredding the waste wind turbine blades into coarse powder and crushing them into fine powder to obtain waste wind turbine blade particles;
[0057] S2. Mixing the waste wind turbine blade particles with wood chips and modified MDI glue and then performing molding to obtain the composite molded product.
[0058] As an optional embodiment of the preparation method of the present invention, in step S1, the thickness of the waste wind turbine blades is not more than 8 cm (such as 8 cm, 7 cm, 6 cm, 5 cm, 4 cm, 3 cm, 2 cm, 1 cm, etc.); and / or the particle size of the waste wind turbine blade particles is 10-20 mm (such as 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, etc.).
[0059] As an optional embodiment of the preparation method of the present invention, in step S2, the particle size of the wood chips is 10-20 mm (such as 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, etc.); and / or the modified MDI glue, measured by mass fraction, includes 26-49% diphenylmethane diisocyanate, 50-64% polymethylene polyphenyl polyisocyanate and 1-10% urethane modified isocyanate.
[0060] As an optional embodiment of the preparation method of the present invention, in step S2, during mixing, the total moisture content of the waste wind turbine blade particles and wood chips is 10-15% (such as 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, etc.); further, when the total moisture content is lower than 10%, water is added during mixing to make the total moisture content at least 10%; when the total moisture content is higher than 15%, the total moisture content is at most 15% by drying and reducing water before mixing.
[0061] As an optional implementation of the preparation method of the present invention, in step S2, the weight ratio of the waste wind turbine blade particles, wood chips and modified MDI glue is (0.5-0.9): (0.05-0.45): (0.03-0.05), and the total of the three is 1.
[0062] According to a third aspect of the present invention, a system for preparing the above-mentioned composite molded products comprises a feeding conveyor, a shredder, a crusher, a dryer, a storage bin, a glue mixer and a molding machine connected in sequence along the material output direction; wherein the storage bin comprises a blade storage bin and a wood chip storage bin.
[0063] The preparation system of the present invention is professionally used for the production of mixed materials such as wind turbine blades and sawdust. A shredder is used to make the first coarse powder of the waste wind turbine blades, and then the waste wind turbine blade materials after the coarse powder are passed through a pulverizer for the second fine powder to obtain waste wind turbine blade particles with a particle size of 10-20 mm for standby use. If the particle size of the sawdust is too large, the aforementioned shredder and pulverizer can be used to crush it to obtain sawdust with a particle size of 10-20 mm for standby use.
[0064] In the process of preparing materials at the front end of the mixing machine, two types of storage bins are equipped, namely, blade storage bin and wood chip storage bin. According to the raw material ratio required for production, they are selected respectively. When blade materials are needed, the feed port of the dryer leading to the blade bin is opened, and the required blade materials will automatically enter the blade storage bin. When wood chip materials are needed, the feed port of the dryer leading to the wood chip bin is opened, and the required wood chip materials will automatically enter the wood chip storage bin. At this time, the dryer plays the role of conveying raw materials.
[0065] When mixing the glue, it is also necessary to ensure that the total moisture content of the sawdust and leaves is 10-15%. If it is lower than 10%, an appropriate amount of water is introduced through the water inlet pipe of the glue mixer during mixing to make the total moisture content of the sawdust and leaves at least 10%; if it is higher than 15%, the sawdust and leaves are dried and dehydrated in a dryer before mixing the glue or storing in the storage bin, so that the total moisture content of the sawdust and leaves is at most 15%. The dried raw materials will be buffered in their respective silos.
[0066] When production begins, the glue mixer is started, and the two raw materials will automatically enter the glue mixer in a set ratio. The glue mixer also uses a large-scale spraying method to spray the glue into the raw materials and spread it all over them to ensure uniform mixing. After uniform mixing, the glue mixer automatically stops working and automatically discharges the materials. The glue mixer includes components such as a floor scale, conveyor, glue sprayer, electronic scale, and water inlet pipe, which are accurate in weighing and easy to operate.
[0067] As an optional embodiment of the preparation system of the present invention, the shredder, pulverizer, dryer and storage bin are all provided with dust removal devices;
[0068] And / or, the dryer and the molding machine are further connected via a mold temperature controller;
[0069] And / or, a buffer silo is provided between the shredder and the pulverizer;
[0070] And / or, the dryer is a rotor dryer.
[0071] The dust removal device of the present invention can be a pulse dust removal system in the prior art, or it can be other devices capable of dust removal, as long as dust pollution can be avoided. The mold temperature controller uses oil as a temperature transfer medium to transfer heat to the dryer and / or molding machine that needs to be heated, avoiding the high energy consumption of electric heating. The setting of the buffer silo is used to buffer the materials between the shredder and the grinder to ensure an efficient and high-quality production rhythm. The preparation method and system of the present invention use retired wind turbine blades as raw materials to produce composite molded pallets, composite building formwork and other products, realizing the resource application of retired wind blade composite materials. At the same time, in the process of recycling and utilizing wind turbine blades, the emission standards prescribed by the state are strictly controlled and implemented, and no wastewater, waste gas, or waste residue is generated, which will not have a significant impact on the regional ecological environment.
[0072] The present invention will be described in detail below through examples. The modified MDI glue used in the examples of the present invention is WANNATE 9131FC produced by Wanhua Chemical Group Co., Ltd., and the mass percentages of various components in the glue are: 26-49% diphenylmethane diisocyanate, 50-64% polymethylene polyphenyl polyisocyanate and 1-10% urethane modified isocyanate.
[0073] Example 1
[0074] A method for preparing a composite material molded pallet, comprising:
[0075] S1. Waste wind turbine blades with a thickness of no more than 8 cm and a matrix material of epoxy resin and glass fiber are transported to a wind turbine blade shredder through a feeding conveyor to be shredded into coarse powder, and then the coarse powder is buffered in a buffer silo, and then pulverized into fine powder in a pulverizer. After the fine powder is pulverized, waste wind turbine blade particles with a particle size of 10-20 mm are obtained, and stored in a blade storage silo for standby use;
[0076] S2. The spare waste wind turbine blade particles, the waste wood chips with a particle size of 10-20 mm stored in the wood chip storage bin, and the modified MDI glue are uniformly mixed in a glue mixer at a mass ratio of 0.8:0.16:0.04. During mixing, the total moisture content of the waste wind turbine blade particles and the wood chips is 15%. After mixing, the glue mixer automatically stops mixing and automatically discharges the material into the molding machine. The molding parameters of the molding machine are: temperature 150°C; curing time 180s; use pressure 15MPa; after molding, a composite material molded pallet is obtained.
[0077] In the preparation system used in this embodiment, the shredder, pulverizer, rotor dryer and two storage bins are all equipped with pulse dust removal systems; and the rotor dryer and the molding machine are also connected through a mold temperature controller, and the oil medium of the mold temperature controller provides the rotor dryer and the molding machine with the required heating temperature. The rotor dryer is used to transport and / or dry waste wind turbine blade particles and waste wood chips. The specific process flow chart is as follows Figure 1 shown.
[0078] The composite molded pallet obtained in this embodiment is 1.2 m long, 1 m wide, 15 cm high, and weighs 22 kg. Its structure is as follows: Figure 2 shown.
[0079] Example 2
[0080] The obtained pallet differs from Example 1 only in that the weight ratio of the waste wind turbine blade particles, wood chips and modified MDI glue is 0.5:0.45:0.05;
[0081] The molding parameters of the molding machine are: the total moisture content of the waste wind turbine blade particles and the wood chips is 10%; the temperature is 135° C.; the curing time is 300 s; and the operating pressure is 20 MPa.
[0082] The rest of the settings are the same as those in Example 1.
[0083] Example 3
[0084] The obtained pallet differs from Example 1 only in that the weight ratio of the waste wind turbine blade particles, wood chips and modified MDI glue is 0.9:0.07:0.03;
[0085] The molding parameters of the molding machine are: the total moisture content of the waste wind turbine blade particles and the wood chips is 12%; the temperature is 155° C.; the curing time is 240s; and the operating pressure is 18MPa.
[0086] The rest of the settings are the same as those in Example 1.
[0087] Comparative Example 1
[0088] The obtained pallet differs from Example 3 only in that the weight ratio of the waste wind turbine blade particles to the modified MDI glue is 0.97:0.03, and does not contain wood chips.
[0089] The rest of the settings are the same as those in Example 3.
[0090] Comparative Example 2
[0091] The obtained pallet differs from that of Example 2 only in that the modified MDI glue is replaced by a single diphenylmethane diisocyanate.
[0092] The rest of the settings are the same as those in Example 2.
[0093] Comparative Example 3
[0094] The obtained pallet differs from Example 2 only in that the weight ratio of the waste wind turbine blade particles, wood chips and modified MDI glue is 0.4:0.55:0.05.
[0095] The rest of the settings are the same as those in Example 2.
[0096] Comparative Example 4
[0097] The only difference between the obtained tray and Example 2 is that the particle size of the waste wind turbine blade particles is greater than 0 and less than 10 mm.
[0098] The rest of the settings are the same as those in Example 2.
[0099] Comparative Example 5
[0100] The obtained tray is different from Example 2 only in that the particle size of the waste wind turbine blade particles is greater than 20 mm and less than 30 mm.
[0101] The rest of the settings are the same as those in Example 2.
[0102] Comparative Example 6
[0103] The obtained pallet is different from Example 2 only in that the particle size of the wood chips is greater than 0 and less than 10 mm.
[0104] The rest of the settings are the same as those in Example 2.
[0105] Comparative Example 7
[0106] The obtained pallet is different from Example 2 only in that the particle size of the wood chips is greater than 20 and less than 30 mm.
[0107] The rest of the settings are the same as those in Example 2.
[0108] Comparative Example 8
[0109] The obtained tray differs from that of Example 2 only in that the total moisture content of the waste wind turbine blade particles and the wood chips is 8%.
[0110] The rest of the settings are the same as those in Example 2.
[0111] Comparative Example 9
[0112] The obtained tray is different from Example 2 only in that the total moisture content of the waste wind turbine blade particles and the wood chips is 16%.
[0113] The rest of the settings are the same as those in Example 2.
[0114] Comparative Example 10
[0115] The obtained tray differed from that of Example 2 only in that the temperature of the molding machine was 130°C.
[0116] The rest of the settings are the same as those in Example 2.
[0117] Comparative Example 11
[0118] The obtained tray differs from that of Example 2 only in that the curing time of the molding machine is 170 s.
[0119] The rest of the settings are the same as those in Example 2.
[0120] Comparative Example 12
[0121] The obtained pallet differs from that of Example 2 only in that the pressure used by the molding machine is 14 MPa.
[0122] The rest of the settings are the same as those in Example 2.
[0123] Detection
[0124] The pallets obtained in the examples and comparative examples were sampled as specimens for fork lifting test, stacking test and formaldehyde emission test. The fork lifting test was carried out in accordance with GB / T 4995-2014 and GB / T 4996-2014. In a test environment of 15°C and 27% RH, the top deck of the specimen was placed upward on support bars with a spacing of 570 mm, and a loading bar was placed above the specimen. The test direction is the long direction. The downward pressing speed of the upper pressing plate of the pressure testing machine is 12.7 mm / min. The load is gradually increased until the specimen is damaged. The load value U1 at this time is recorded as the limit load.
[0125] The stacking test is carried out in accordance with GB / T 4995-2014 and GB / T 4996-2014. In the test environment of 15℃ and 27%RH, the top plate of the sample is placed upward at the center of the press, and a loading bar is placed above the top plate. The hole width is L1. The test direction is the long direction. The downward pressing speed of the upper plate of the pressure testing machine is 12.7mm / min. The load is gradually increased until the sample is damaged or causes a deflection value of L1×6%. The load value U2 at this time is recorded as the limit load.
[0126] The formaldehyde emission is tested according to the dryer method of GB / T 17657-2013.
[0127] The test equipment is shown in Table 1 below, and the test results are shown in Table 2 below.
[0128] Table 1
[0129]
[0130] Table 2
[0131]
[0132] As shown in Table 2, the pallets obtained in Examples 1-3 have smooth surfaces, are not prickly, and are extremely convenient to use, thus avoiding the inconvenience of using the pallet with a prickly surface. In addition, in terms of load-bearing capacity, the dynamic load is greater than 2.7 tons and the static load is greater than 14 tons, which not only meets the use requirements but also has excellent load-bearing capacity, and the cost is greatly reduced compared with general pallets with equivalent load-bearing capacity.
[0133] By comparing Example 3 with Comparative Example 1, and by comparing Example 2 with Comparative Example 2, it can be seen that the sawdust and modified MDI glue in the pallet components of the present invention both have the effect of increasing the load and smoothing the surface. In particular, the sawdust component, by adding a small amount, can increase the load and make the surface smooth. Further, by comparing Example 2 with Comparative Example 3, it can be seen that when preparing the pallet of the present invention, the weight ratio of waste wind turbine blades, sawdust and modified MDI glue is further controlled within the range of (0.5-0.9): (0.05-0.45): (0.03-0.05), so that the content of waste wind turbine blades is higher than the content of sawdust, and the resulting pallet has outstanding bearing capacity. By comparing Example 2 with Comparative Examples 4-7, it can be seen that when preparing the pallet of the present invention, the particle size of the waste wind turbine blade particles is further controlled to be 10-20mm, and the particle size of the sawdust is 10-20mm, and the two can be well matched with each other, so that the glass fibers in the waste wind turbine blades are covered and wrapped by the sawdust, the surface of the pallet is smooth and not prickly, and the bearing capacity of the pallet can be improved. By comparing Example 2 with Comparative Examples 8 and 9, it can be seen that when preparing the pallet of the present invention, further controlling the total moisture content of the waste wind turbine blades and wood chips can better cooperate with the modified MDI glue to improve the carrying capacity of the pallet. By comparing Example 2 with Comparative Examples 10-12, it can be seen that when preparing the pallet of the present invention, the temperature, curing time and use pressure of the molding machine cannot be too small, which will lead to a reduction in the carrying capacity of the pallet. When the temperature, curing time and use pressure are too large in actual production, it will cause unnecessary energy consumption and low production efficiency.
[0134] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A composite molded product, characterized in that: The composite molded product is obtained by mixing waste wind turbine blades, wood chips and modified MDI glue and then molding them, and the matrix material of the waste wind turbine blades is epoxy resin and glass fiber; The weight ratio of the waste wind turbine blades, wood chips and modified MDI glue is (0.5-0.9): (0.05-0.45): (0.03-0.05), and the total of the three is 1; The modified MDI glue comprises, by mass fraction, 26-49% of diphenylmethane diisocyanate, 50-64% of polymethylene polyphenyl polyisocyanate and 1-10% of urethane modified isocyanate; The composite material molded product is one of a molded pallet, a cable drum, a fence, a high-speed guardrail, and a city municipal environmental protection manhole cover; The total moisture content of the waste wind turbine blades and sawdust is 10-15%; The waste wind turbine blades are mixed with sawdust and modified MDI glue in the form of particles and then molded, and the particle size of the waste wind turbine blades is 10-20 mm; The particle size of the sawdust is 10-20 mm; The molding temperature is 135-155°C; The curing time of the molding is 180 to 300 seconds; The molding pressure is 15-20 MPa.
2. The composite molded product according to claim 1, characterized in that: The molding temperature is 150°C; And / or, the curing time of the molding is 180s.
3. A method for preparing a composite molded product as claimed in any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: S1. Shredding the waste wind turbine blades into coarse powder and crushing them into fine powder to obtain waste wind turbine blade particles; S2. Mixing the waste wind turbine blade particles with wood chips and modified MDI glue and then performing molding to obtain the composite molded product.
4. The preparation method according to claim 3, characterized in that: In step S1, the thickness of the waste wind turbine blades is not greater than 8 cm.
5. The preparation method according to claim 3, characterized in that: In step S2, when the total moisture content of the waste wind turbine blade particles and sawdust is lower than 10%, water is added during mixing to make the total moisture content at least 10%; when the total moisture content of the waste wind turbine blade particles and sawdust is higher than 15%, drying and water reduction are performed before mixing to make the total moisture content at most 15%.
6. A system for preparing a composite molded product as claimed in any one of claims 1 to 2, characterized in that: The preparation system includes a feeding conveyor, a shredder, a crusher, a dryer, a storage bin, a glue mixer and a molding machine which are sequentially connected along the material output direction; wherein the storage bin includes a blade storage bin and a wood chip storage bin.
7. The preparation system according to claim 6, characterized in that: The shredder, crusher, dryer and storage bin are all equipped with dust removal devices; And / or, the dryer and the molding machine are further connected via a mold temperature controller; And / or, a buffer silo is provided between the shredder and the pulverizer; And / or, the dryer is a rotor dryer.