Carbon materials and their preparation methods, hydrogenation reaction catalysts and their preparation methods and applications
By modifying carbon materials with single-atom Cr and noble metals, the resulting catalyst significantly improves the hydrogenation reaction activity of the anode in alkaline fuel cells, solving the problem of large amounts of noble metals used in alkaline membrane fuel cells and achieving a highly efficient alkaline hydrogenation reaction.
Patent Information
- Application Number
- CN202311712462.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-13
AI Technical Summary
The slow kinetics of hydrogen oxidation at the anode of alkaline membrane fuel cells necessitate the use of large amounts of platinum group metal catalysts, increasing costs and limiting their development.
Using carbon materials as a support, a catalyst is formed by modifying it with single-atom Cr and noble metals (such as Pt, Pd, Ir, Ru, Rh). The single-atom Cr improves the interfacial double-layer structure and enhances the hydrogenation activity of noble metals in an alkaline environment.
It significantly improves the alkaline hydroxide activity of precious metal catalysts, reduces the amount of precious metals used in anode catalysts, and enhances the power output performance of alkaline fuel cells.
Smart Images

Figure CN117701036B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts, specifically to carbon supports and their preparation methods, hydrogenation reaction catalysts and their preparation methods and applications. Background Technology
[0002] With the global population continuing to grow, energy demand is increasing, climate change is becoming increasingly urgent, and concerns about future energy security are growing daily. Therefore, we urgently need to diversify our energy sources and reduce our dependence on fossil fuels.
[0003] Low-temperature proton exchange membrane fuel cells (PEMFCs) are the mainstream type of fuel cell for vehicles and are an important device for realizing a hydrogen economy. Although the development of PEMFCs is nearing maturity, they heavily rely on platinum group metals, and the slow oxygen reduction kinetics at the cathode require the use of large amounts of Pt-based catalysts. This results in high costs for PEMFCs and limits their commercialization.
[0004] In recent years, with the continuous development of alkaline anion exchange membranes, alkaline ionomers, and alkaline battery assembly processes, alkaline membrane fuel cells have gradually shown promising prospects and have become a potential replacement for proton exchange membrane fuel cells. Thanks to the mild reaction conditions of alkaline membrane fuel cells, non-precious metals can be used to replace Pt-based catalysts for the cathode oxygen reduction catalyst. Ag-based materials, MnCo oxides, and Fe-NC materials have all exhibited good activity.
[0005] However, the hydrogen oxidation reaction (HOR) at the anode exhibits a strong pH dependence; under alkaline conditions, the HOR kinetics of platinum group metal catalysts are generally 2–3 orders of magnitude slower than under acidic conditions. Therefore, to achieve high power output, alkaline membrane fuel cells require a large amount of platinum group metal catalyst at the anode, with a noble metal loading approximately 10 times that of proton exchange membrane fuel cells with similar performance. This leads to a significant increase in anode catalyst costs and hinders the development of alkaline membrane fuel cells.
[0006] Therefore, developing highly efficient alkaline hydroxide catalysts with activity close to that of Pt under acidic conditions, thereby significantly reducing anode costs, will be of great significance to the development of alkaline membrane fuel cells. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of existing technologies in alkaline hydroxide reaction catalysts, which have low activity.
[0008] To achieve the above objectives, a first aspect of the present invention provides a method for preparing carbon materials, comprising:
[0009] (1) At temperature T1, carbon raw material is contacted and mixed with strong acid solution, and the material I obtained after contact mixing is separated to obtain carbon oxide precursor material. T1 is 50-100℃, and the carbon raw material is selected from at least one of carbon black, carbon nanotubes, and graphene.
[0010] (2) The carbon oxide precursor is dispersed in water and then filtered, and the resulting carbon material is dried to obtain the carbon material.
[0011] A second aspect of the invention provides a carbon material prepared by the method described in the first aspect.
[0012] A third aspect of the present invention provides a hydrogenation reaction catalyst comprising a support and a metal active component, wherein the support is the carbon material described in the second aspect; the metal active component comprises a second metal element and a first metal element; the first metal element is selected from at least one of Pt, Pd, Ir, Ru, and Rh; the second metal element is selected from at least one of Cr, V, Mn, Fe, Co, Ni, Cu, and Zn; and the first metal element is distributed on the carbon material in a single-atom dispersed state.
[0013] A fourth aspect of the present invention provides a method for preparing a catalyst for a hydrogenation reaction, the method comprising:
[0014] S1: In a solution environment, the active metal source and the support are mixed to obtain a catalyst precursor; the support is the carbon material described in the second aspect of the present invention.
[0015] S2: Reduce the catalyst precursor;
[0016] The active metal source is selected from substances capable of providing active metal components, wherein the active metal components contain a second metal element and a first metal element, wherein the first metal element is selected from at least one metal element selected from Pt, Pd, Ir, Ru, and Rh; and the second metal element is selected from at least one metal element selected from Cr, V, Mn, Fe, Co, Ni, Cu, and Zn.
[0017] The fifth aspect of the present invention provides a hydrogenation reaction catalyst prepared by the method described in the fourth aspect.
[0018] The sixth aspect of the invention provides the use of the hydroxide reaction catalyst described in the third and / or fifth aspects in an alkaline hydrogen oxidation reaction.
[0019] Alkaline membrane fuel cells have slow anode reaction kinetics and require a large amount of platinum group metal catalysts to support high power output. The carbon material catalyst provided in this invention has activity similar to that of platinum high-efficiency catalysts in acidic environments.
[0020] In particular, the present invention provides a strategy for improving the alkaline hydroxide reaction activity of noble metal catalysts by modifying carbon supports with Cr single atoms, which has a general effect on improving the alkaline hydroxide reaction activity of Pt group metals.
[0021] The hydrogenation catalyst provided by this invention contains synergistic metal nanoclusters and metal single-atom modified carbon supports; the single-atom modified carbon supports can improve the interfacial electric double layer structure and significantly enhance the alkaline hydrogen oxidation activity of active metals, especially Pt group metals (Pt, Rh, Pd, Ir, Ru).
[0022] The hydrogen oxidation catalyst provided by this invention can efficiently catalyze the hydrogen oxidation reaction in an alkaline medium.
[0023] In a particularly preferred embodiment, the present invention also provides a Rh group cluster / Cr single-atom carbon support composite catalyst (RhCr NCs / SAC), which exhibits an activity more than 100 times higher than that of commercial Pt-based catalysts. Alkaline membrane fuel cells assembled using this catalyst can achieve high efficiency with only 10 μg of fuel. Rh / cm 2 Under the conditions of an anode catalyst, it can provide 1.86 W cm⁻¹ -2 Peak power density.
[0024] After analysis, the inventors of this invention believe that the enhanced activity of the Rh-based catalyst proposed in this invention may be due to two factors: firstly, the regulation of the electronic structure of Rh by the Cr element, and secondly, the regulation of the interfacial water structure in the electric double layer of the Rh surface by the aforementioned Cr single-atom modified support. Attached Figure Description
[0025] Figure 1 These are TEM images of different noble metal / single-atom Cr-modified carbon support catalysts obtained in the examples of the present invention; wherein, a represents RhCr NCs / SAC, b represents RuCr NCs / SAC, c represents IrCr NCs / SAC, d represents PtCr NCs / SAC, and e represents PdCr NCs / SAC.
[0026] Figure 2 These are examples of HAADF-STEM, EDS mapping diagrams, and structural schematic diagrams of RhCr NCs / SAC obtained in this invention, where a is the HAADF-STEM diagram, b is the EDS mapping diagram, and c is the structural schematic diagram.
[0027] Figure 3The polarization curves are obtained by testing different noble metal / single-atom Cr-modified carbon support catalysts obtained in Examples 1 to 5 of the present invention in 0.1M KOH saturated with hydrogen.
[0028] Figure 4 yes Figure 3 The mass ratio exchange currents of a series of different noble metal catalysts shown are tested in hydrogen-saturated 0.1M KOH, and their performance is compared with that of the corresponding carbon-supported noble metal nanoparticles.
[0029] Figure 5 The polarization curves are obtained by testing RhCr catalysts with different molar contents in hydrogen-saturated 0.1M KOH in examples of this invention.
[0030] Figure 6 yes Figure 5 The mass ratio exchange currents of a series of catalysts shown were obtained by testing in 0.1M KOH saturated with hydrogen.
[0031] Figure 7 The polarization curves of RhCr NCs / SAC were obtained by testing in 0.1M KOH saturated with hydrogen. Its hydrogen oxidation performance is compared with that of commercial Pt / C (40wt%) and PtRu / C (40wt% Pt, 20wt% Ru) measured in 0.1M KOH saturated with hydrogen.
[0032] Figure 8 The polarization curves of the alkaline membrane electrode assembled with RhCr NCs / SAC under hydrogen pump conditions are shown. Its hydrogen oxidation performance is comparable to that of commercially available alkaline membrane electrodes assembled with Pt / C (40wt%) and PtRu / C (40wt% Pt, 20wt% Ru).
[0033] Figure 9 This is a performance diagram of an alkaline membrane fuel cell with low anode catalyst loading assembled with RhCr NCs / SAC obtained in an example of the present invention. Its battery performance is compared with that of commercial alkaline membrane fuel cells assembled with the same loading of Pt / C (40wt%) and PtRu / C (40%wtPt, 20%wtRu).
[0034] Figure 10 yes Figure 9 The graph shown compares the performance and catalyst loading of fuel cells with those of alkaline membrane fuel cells assembled with existing high-performance hydroxide catalysts.
[0035] Figure 11These are TEM images of catalysts formed by modifying supports with metallic Rh with single-atom transition metals V, Mn, Fe, Co, Ni, Cu, and Zn. In the images, a represents RhV NCs / SAC, b represents RhCr NCs / SAC, c represents RhMn NCs / SAC, d represents RhFeNCs / SAC, e represents RhCo NCs / SAC, f represents RhNi NCs / SAC, g represents RhCu NCs / SAC, and h represents RhZn NCs / SAC.
[0036] Figure 12 These are the alkaline hydrogen oxidation polarization curves of the metal Rh / different transition metal single-atom modified carbon support catalysts obtained in Examples 5-12.
[0037] Figure 13 yes Figure 12 The mass ratio exchange currents of a series of different transition metal catalysts shown are tested in hydrogen-saturated 0.1M KOH, and their performance is compared with that of Rh / C nanoparticles.
[0038] Figure 14 This is a graph showing the electrocatalytic performance of RhCr NCs / SAC.
[0039] Figure 15 The X-ray absorption spectra of single-atom Cr-modified carbon supports in RhCr NCs / SAC are shown, where a is the near-edge X-ray absorption spectrum and b is the extended fine X-ray absorption spectrum. Detailed Implementation
[0040] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0041] As previously described, a first aspect of the present invention provides a method for preparing carbon materials, comprising:
[0042] (1) At temperature T1, carbon raw material is contacted and mixed with strong acid solution, and the material I obtained after contact mixing is separated to obtain carbon oxide precursor material. T1 is 50-100℃, and the carbon raw material is selected from at least one of carbon black, carbon nanotubes, and graphene.
[0043] (2) The carbon oxide precursor is dispersed in water and then filtered, and the resulting carbon material is dried to obtain the carbon material.
[0044] Preferably, in step (1), the strong acid solution is selected from at least one of nitric acid, sulfuric acid, and potassium permanganate.
[0045] Preferably, in step (1), the H ion concentration in the strong acid solution is 11-14 mol / L.
[0046] In a preferred embodiment, in step (1), the weight ratio of the carbon raw material to the strong acid solution is 1:90-120.
[0047] Preferably, in step (1), the carbon raw material is carbon black and the strong acid solution is nitric acid.
[0048] Preferably, in step (1), the carbon raw material is KB-300J type carbon black; the strong acid solution is an aqueous solution of nitric acid with a concentration greater than 50 wt%. The inventors have found that, under this preferred condition, the carbon support obtained by the present invention has suitable oxygen vacancies and significantly better stability.
[0049] More preferably, the concentration of the nitric acid aqueous solution is 60-65 wt%.
[0050] According to a preferred embodiment, in step (1), before the contact mixing is performed, the carbon raw material and the strong acid solution are first subjected to ultrasonic pretreatment, and then the pretreated mixed solution is subjected to the contact mixing.
[0051] Preferably, the frequency of the ultrasound is 30kHz-50kHz.
[0052] Preferably, in step (1), the contact mixing temperature is 70-90℃ (that is, T1 is 70-90℃) and the time is 0.2-4h.
[0053] In a preferred embodiment, in step (1), the separation process is carried out by centrifugal separation.
[0054] According to a preferred embodiment, the centrifugal separation conditions include: a rotation speed of 5000-10000 rpm and a time of 3-10 min.
[0055] It should be noted that in step (2), the solution environment refers to an environment in which a solution exists, which may also contain solid substances, as long as a solution exists.
[0056] Preferably, in step (2), the drying process is carried out by freeze-drying. The inventors have found that the carbon support of the present invention in this preferred embodiment has a loose structure, which is significantly advantageous for subsequent applications (e.g., catalyst preparation).
[0057] More preferably, the freeze-drying conditions include: a temperature of -60°C to -70°C and a time of 12-24 hours.
[0058] This invention does not have any particular requirements for the specific operation method of freeze-drying, and those skilled in the art can use the operations known in the art.
[0059] According to a particularly preferred embodiment, the method for preparing the carbon support includes:
[0060] (A1) Under ultrasonic conditions, carbon raw material is first mixed with a strong acid solution to obtain mixture I; mixture I is heated at 50-100°C to obtain material I; the carbon raw material is selected from at least one of carbon black, carbon nanotubes, and graphene;
[0061] (A2) The material I is centrifuged and the resulting filter residue is washed to obtain the carbon oxide precursor material;
[0062] (A3) The carbon oxide precursor is dispersed in water and then filtered to obtain carbon material;
[0063] (A4) The carbon material is freeze-dried to obtain the carbon material.
[0064] Preferably, the temperature of the first mixing is 10-30°C.
[0065] Preferably, in step (A1), the ultrasonic conditions are the same as those described in step (1) of the present invention.
[0066] Preferably, in step (A2), the centrifugal separation conditions are the same as those described in step (1) of the present invention.
[0067] It should be noted that in step (A1), the total time of the first mixing and the heating reaction is the contact mixing time in step (1) of the present invention.
[0068] As previously stated, a second aspect of the present invention provides a carbon material prepared by the method described in the first aspect.
[0069] As previously described, a third aspect of the present invention provides a hydrogenation reaction catalyst comprising a support and a metal active component, wherein the support is the carbon material described in the second aspect; the metal active component comprises a second metal element and a first metal element; the first metal element is selected from at least one of Pt, Pd, Ir, Ru, and Rh; the second metal element is selected from at least one of Cr, V, Mn, Fe, Co, Ni, Cu, and Zn; and the first metal element is distributed on the carbon material in a single-atom dispersed state.
[0070] Preferably, the loading of the metal active component is 0.5-0.8 wt%, based on the total weight of the carbon material.
[0071] Preferably, the molar ratio of the second metal element to the first metal element is 1:99 to 40:60.
[0072] Preferably, the second metal element is distributed on the carrier in the form of metal clusters.
[0073] Preferably, the average particle size of the metal clusters is not greater than 2 nm.
[0074] Preferably, the content of the support is 90-97 wt% based on the total weight of the catalyst, with the balance being the active metal component.
[0075] According to a particularly preferred embodiment, in the hydroxide reaction catalyst, the active metal component contains Cr and a first metal element, wherein the first metal element is Rh, and the molar ratio of Cr to Rh is from 1:99 to 40:60. For example, the molar ratio of Rh to Cr is 99:1, 95:5, 90:10, 80:20, 75:25, 70:30, 65:35, 60:40, and most preferably 70:30.
[0076] As previously described, a fourth aspect of the present invention provides a method for preparing a catalyst for a hydrogenation reaction, the method comprising:
[0077] S1: In a solution environment, the active metal source and the support are mixed to obtain a catalyst precursor; the support is the carbon material described in the second aspect of the present invention.
[0078] S2: Reduce the catalyst precursor;
[0079] The active metal source is selected from substances capable of providing active metal components, wherein the active metal components contain a second metal element and a first metal element, wherein the first metal element is selected from at least one metal element selected from Pt, Pd, Ir, Ru, and Rh; and the second metal element is selected from at least one metal element selected from Cr, V, Mn, Fe, Co, Ni, Cu, and Zn.
[0080] The present invention does not have specific requirements for the specific substance in the active metal source, as long as it can provide an active metal element. In a particularly preferred embodiment, the active metal source is at least one of a salt (e.g., chloride), oxide, or sulfide that can provide the active metal element of the present invention.
[0081] Preferably, the amount of the active metal source is such that the molar ratio of the second metal element to the first metal element in the hydrogenation reaction catalyst is 1:99 to 40:60; more preferably, it is 25:75 to 35:65.
[0082] It should be noted that in step S1, the solution environment refers to an environment in which a solution exists, which may also contain solid substances, as long as a solution is present.
[0083] In a preferred embodiment, the mixing conditions in step S1 include: a temperature of 30-80°C and a time of 0.1-5 hours.
[0084] Preferably, in step S1, the mixing process is performed under ultrasonic conditions.
[0085] Preferably, the frequency of the ultrasound is 30kHz-50kHz.
[0086] Preferably, the method of the present invention further includes, after performing step S1, subjecting the obtained catalyst precursor to rotary evaporation and drying treatment in sequence, and then using the dried catalyst precursor in step S2.
[0087] It should be noted that the present invention does not have any special requirements for the rotary evaporation process, and those skilled in the art can perform it according to the operations known in the art.
[0088] Preferably, after step S1, the drying process is carried out at a temperature of 40-70°C.
[0089] The method of the present invention may also include various post-processing methods known in the art, such as solvent removal, etc., which will not be described in detail here, and should not be construed as a limitation of the present invention by those skilled in the art.
[0090] The present invention does not have any special requirements for the specific operation method of the restoration process in step S2, and those skilled in the art can perform it according to the operations known in the art.
[0091] In a particularly preferred embodiment, step S2 includes performing the reduction treatment by: in the presence of a reducing atmosphere, programming the temperature of the catalyst precursor to T2 and maintaining it at T2 for time t.
[0092] Preferably, the temperature T2 is 200-600℃, and the time t is 1-8h.
[0093] In a particularly preferred embodiment, the rate of temperature increase is 5-15 °C / min.
[0094] According to a particularly preferred embodiment, the active metal component contains Rh and Cr. More preferably, the amount of the active metal source is such that the molar ratio of Cr to Rh in the prepared catalyst is 1:99 to 40:60. For example, the amount of the active metal source is such that the molar ratio of Rh to Cr in the prepared catalyst is 99:1, 95:5, 90:10, 80:20, 75:25, 70:30, 65:35, 60:40, and most preferably 70:30. The Rh-based highly active alkaline hydroxide catalyst provided by this invention has Rh metal clusters and a single-atom Cr carbon support. Compared with traditional commercial Pt-based and Ru-based catalysts, the catalyst provided by this invention exhibits significantly improved electrocatalytic performance, and the noble metal loading used in the anode of alkaline fuel cells can be reduced by 1-2 orders of magnitude.
[0095] As previously stated, the fifth aspect of the present invention provides a hydrogenation reaction catalyst prepared by the method described in the fourth aspect.
[0096] In particularly preferred cases, the carbon black support modified with single-atom Cr provided by the present invention can grow ultra-small noble metal nanoclusters (average particle size of 1nm to 2nm). Furthermore, the carbon support modified with single-atom Cr is relatively hydrophilic. Due to the size matching between the single-atom support and the cluster, the single-atom Cr site can affect the water double layer structure on the surface of the noble metal cluster. The resulting catalyst has enhanced alkaline hydrogen oxidation activity compared with noble metal nanoparticles supported by traditional supports.
[0097] As previously stated, the sixth aspect of the present invention provides the use of the hydroxide reaction catalyst described in the third and / or fifth aspects in the alkaline hydrogen oxidation reaction.
[0098] The hydrogenation catalyst provided by this invention exhibits high activity under alkaline conditions.
[0099] The inventors of this invention have discovered that the catalyst of this invention exhibits significantly enhanced alkaline hydroxide activity compared to commercial Rh / C catalysts.
[0100] The present invention will be described in detail below through examples. In the following examples, unless otherwise specified, all raw materials and instruments used are commercially available products.
[0101] KB-300J: Purchased from Suzhou Shengernuo Technology Co., Ltd.
[0102] IrCl3·xH2O: Purchased from Beijing Innocare Technology Co., Ltd., item number A66777.
[0103] RuCl3·xH2O: Purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number R294711.
[0104] RhCl3·xH2O: Purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd., item number 206261.
[0105] Catalyst characterization
[0106] The morphology of the prepared catalyst was analyzed using a HITACHI HT7700 electron transmission microscope.
[0107] The structure of the catalyst at the atomic scale was characterized using a FEI-Titan Cubed Themis G2 300 scanning transmission electron microscope.
[0108] The composition of the catalyst was determined using a Thermo-Fisher ICPS-6300 inductively coupled plasma atomic emission spectrometer.
[0109] The CHI 760e electrochemical workstation was used to test the hydrogenation reaction of the corresponding catalyst.
[0110] The performance of alkaline membrane fuel cells was tested using the Scribner 850e battery system.
[0111] The hydrogen pump was tested using a Solartron ModuLab XM workstation.
[0112] Example 1: Preparation of a bimetallic catalyst (PtCr NCs / SAC) with a platinum-chromium ratio of 7:3
[0113] (1) Weigh 1g of KB-300J and disperse it in 100mL of 65wt% nitric acid. Sonicate for 30min (ultrasonic frequency of 40kHz) to obtain a mixed solution. Then react the mixed solution at 80℃ for 1h.
[0114] (2) Pour the solution after the reaction in step (1) into a centrifuge tube, centrifuge at 9000 rpm for 3 min, then wash with water three times, and disperse the carbon obtained in 150 mL of water.
[0115] (3) Filter the mixed solution obtained in step (2);
[0116] (4) Place the filter residue obtained in step (3) in a freeze dryer to freeze dry (temperature -60℃, time 18h) to obtain carbon oxide powder;
[0117] (5) Take 12.95 mg of H2PtCl6·6H2O (first metal source), 2.85 mg of CrCl3·6H2O (second metal source), and 92.16 mg of carbon oxide powder obtained in step (4) and disperse them in water in a 250 mL rotary evaporator flask. Then, sonicate the mixture at 25 °C for 2 h (ultrasonic frequency of 40 kHz). Then, cool the mixture to 10 °C and keep it for 5 min. Perform rotary evaporation on the cooled mixture. After rotary evaporation, dry the sample in a 50 °C oven to obtain the catalyst precursor.
[0118] (6) Take the catalyst precursor obtained in step (5), grind it in a mortar and spread it evenly in a porcelain boat, then place the porcelain boat in a quartz tube, and heat it to 300℃ at a heating rate of 10℃ / min under a hydrogen atmosphere, and keep it under this condition for 4h. The resulting sample is the final catalyst PtCr NCs / SAC. According to the IPC test results, the molar ratio of platinum to chromium in PtCr NCs / SAC is 7:3.
[0119] The bimetallic catalysts in the remaining examples were prepared using the same methods and process conditions as in Example 1, except that the types and amounts of the first and second metal sources were different, as detailed in Table 1.
[0120] Table 1
[0121]
[0122]
[0123] Preparation Example 1
[0124] Figure 4 The preparation methods of Rh / C, Pt / C, Ru / C, Ir / C, and Pd / C used in this study are as follows:
[0125] (1) Take 12.95 mg of H2PtCl6·6H2O and 92.65 mg of KB-300J and disperse them in water in a 250 mL rotary evaporation flask, and sonicate it at 25 °C for 2 h (ultrasonic frequency of 40 kHz). Then cool the mixed solution to 10 °C and keep it for 5 min. Perform rotary evaporation on the cooled mixed solution. After rotary evaporation, place the obtained sample in a 50 °C oven to dry and obtain the catalyst precursor.
[0126] (2) Take the catalyst precursor obtained in step (1), grind it with a mortar and spread it evenly in a porcelain boat, then place the porcelain boat in a quartz tube, and heat it to 300°C at a heating rate of 10°C / min under a hydrogen atmosphere, and keep it under this condition for 4 hours. The resulting sample is the final catalyst Pt / C.
[0127] The remaining Rh / C, Ru / C, Ir / C, and Pd / C were prepared using the same methods and process conditions as described above. The only difference was the amount of metal source and carbon powder used, but the loading of the active metal was 5 wt% for all of them, as shown in Table 2.
[0128] Table 2
[0129]
[0130] Test case
[0131] Rotating disk electrode test method
[0132] 1. Take 1 mg of the catalyst from each example, add 5 μL of 5 wt% Nafion solution, 895.5 μL of anhydrous ethanol and 99.5 μL of aqueous solution, and disperse by ultrasonication to obtain a uniformly dispersed catalyst ink.
[0133] 2. Take 10 μL of the catalyst ink obtained in step 1 and drop it onto the glassy carbon electrode in two portions. Use the rotating disk electrode method to test the catalyst and keep the rotation speed at 1600 rpm. Test the catalyst in a hydrogen-saturated 0.1 M KOH solution. Use linear voltammetry to collect the hydrogen oxidation polarization curve, control the potential to scan from -0.2 V to 0.8 V and set the scan rate to 5 mV / s.
[0134] Membrane electrode preparation method:
[0135] The membrane electrode was prepared according to the method provided in the literature (Nature Communications 2020, 11, 5651). The specific steps are as follows:
[0136] 1. Using RhCr NCs / SAC as the anode catalyst, weigh 4 mg of RhCr NCs / SAC and 4 mg of carbon black, dissolve the catalyst in 1 ml of isopropanol and 50 μL of aqueous solution, add 127 μL of ionomer solution of 5% PAP-TP-100 ethanol solution, sonicate vigorously for 1 min, and then sonicate in an ice bath for 2 h.
[0137] 2. Using commercial Pt / C (40wt%) as the cathode catalyst, weigh 10mg of Pt / C, dissolve the catalyst in 1ml of isopropanol and 50ul of aqueous solution, add 84ul of 5wt% PAP-TP-100 ethanol solution, and sonicate strongly (20kHz) for 1min, followed by sonication in an ice bath (40kHz) for 2h.
[0138] 3. The ultrasonically dispersed catalyst ink from steps 1 and 2 was sequentially and symmetrically sprayed onto both sides of the alkaline membrane (PAP-TP-85). The anolyte loading was measured to be 0.011 mg by IPC. Rh / cm 2 The cathode loading was 0.33 mg. Pt / cm 2 .
[0139] 4. Soak the alkaline membrane coated with catalyst in 3M NaOH solution overnight, then replace the residual NaOH on the surface of the alkaline membrane with ultrapure water, and gently blot the moisture off the surface of the alkaline membrane with lint-free paper.
[0140] 5. Two gas diffusion layers (SGL 29BC) are sandwiched between the two sides of the alkaline membrane to form a membrane electrode assembly (MEA), and the prepared MEA is placed in a 5 cm² area. 2 In the graphite flow field plate with three serpentine channels, the membrane electrode is clamped with a fixture.
[0141] Note: As a comparison with alkaline membrane devices, the above anode catalysts were replaced with commercial PtRu / C and commercial Pt / C, with the loading controlled at 0.01 mg. PGM / cm 2 .
[0142] Hydrogen pump test method:
[0143] The battery clamp with the MEA installed was heated to 80°C, and hydrogen gas was introduced into both the anode and cathode at a flow rate of 500 sccm. The humidification temperature was 80°C, and the back pressure was 100 kPa. The polarization curve of the working electrode from -1V to 1V was recorded using linear voltammetry while maintaining a scan rate of 5 mV / s. The high-frequency impedance at 0V was measured using AC impedance spectroscopy, and the polarization curve was corrected for resistance.
[0144] Alkaline membrane fuel cell testing methods:
[0145] The battery clamp with the MEA installed was heated to 95°C. Hydrogen gas was introduced into the anode at a flow rate of 1000 sccm, the humidification temperature was 92°C, and the back pressure was 200 kPa. Oxygen gas was introduced into the cathode at a flow rate of 500 sccm, the humidification temperature was 95°C, and the back pressure was 250 kPa. The polarization curve of the battery from open-circuit voltage to 0.2V was recorded using the linear voltammetry method.
[0146] result:
[0147] Through characterization, Figure 1 TEM images of bimetallic catalysts formed by platinum group metals Pt, Rh, Pd, Ir, and Ru with single-atom Cr-modified supports, where... Figure 1 In the figures, a represents a TEM image of the RhCr NCs / SAC catalyst provided in Example 5; b represents a TEM image of the RuCr NCs / SAC catalyst provided in Example 4; c represents a TEM image of the IrCr NCs / SAC catalyst provided in Example 3; d represents a TEM image of the PtCr NCs / SAC catalyst provided in Example 1; and e represents a TEM image of the PdCr NCs / SAC catalyst provided in Example 2. As can be seen from the figures, these catalysts all contain 1-2 nm metal clusters and activated carbon supports.
[0148] Figure 2 The figures show the HAADF-STEM and EDS-mapping images of the RhCr NCs / SAC provided in Example 5, where a is the HAADF-STEM image, b is the EDS mapping image, and c is a schematic diagram of the structure. As can be seen from the figures, the catalyst contains Rh metal clusters and single-atom structures distributed on a carbon support at the atomic scale, while Cr atoms are dispersed as single atoms on both the metal clusters and the carbon support. Based on the above information, the schematic diagram of the catalyst's microstructure includes RhCr nanoclusters and RhCr single-atom carbon supports.
[0149] Figure 3 These are the alkaline hydrogen oxidation polarization curves of different noble metal / single-atom Cr-modified carbon support catalysts obtained in Examples 1-5. Figure 3 As can be seen, the alkaline HOR activities of different noble metal / single-atom Cr modified carbon support catalysts are all excellent, among which the RhCr NCs / SAC provided in Example 5 has the best activity.
[0150] Figure 4 It is based on Figure 3 A comparison of the mass ratio exchange current calculated from the polarization curves of each catalyst and the corresponding activity of the metal nanoparticles. Figure 4It is evident that carbon supports modified with single-atom Cr generally enhance the HOR (Hosting Orientation) properties of platinum group metals. Specifically, the RhCr NCs / SAC provided in Example 5 exhibits a 29.5-fold increase in activity compared to Rh / C; the PtCrNCs / SAC provided in Example 1 exhibits a 15.8-fold increase in activity compared to Pt / C; the RuCr NCs / SAC provided in Example 4 exhibits a 17.5-fold increase in activity compared to Ru / C; the IrCr NCs / SAC provided in Example 3 exhibits a 2.3-fold increase in activity compared to Ir / C; and the PdCrNCs / SAC provided in Example 2 exhibits a 2.8-fold increase in activity compared to Pd / C.
[0151] Using the same method and process conditions as in Example 5, a series of RhCr catalysts containing different molar ratios of Rh and Cr were synthesized by adjusting the amounts of the first and second metal sources. The results were obtained using the rotating disk electrode test method provided in the test example. Figure 5 The alkaline oxidation polarization curves of RhCr catalysts with different proportions are shown.
[0152] Figure 6 It is based on Figure 5 The mass ratio exchange current was calculated from the polarization curves of each catalyst. Figure 5 and Figure 6 As can be seen, the RhCr catalysts with different molar ratios of Rh and Cr provided by this invention all exhibit good activity. Furthermore, the mass activity of the catalyst shows a "volcano-like" trend with increasing Cr content; when the molar ratio of Rh to Cr is in the range of 65:35 to 75:25, the performance is significantly higher, with the catalyst having an RhCr ratio of 7:3 exhibiting the best performance.
[0153] Figure 7 The figures show the hydrogen oxidation polarization curves obtained from RhCr NCs / SAC provided in Example 5 with commercial Pt / C (Pt loading 40 wt%) and commercial PtRu / C (Pt loading 40 wt%, Ru loading 20 wt%) in 0.1 M KOH. Figure 7 It can be seen that, under low catalyst loading, the alkaline hydroxide performance of RhCr NCs / SAC provided in Example 5 is significantly better than that of commercial Pt / C and PtRu / C, where Diffusion represents the diffusion mass transfer curve.
[0154] Figure 8The polarization curves of the RhCr NCs / SAC provided in Example 5 during hydrogen pump testing (HEM represents a hydroxide exchange membrane fuel cell) are shown, with Pt / C (Pt loading of 40 wt%) and PtRu / C (Pt loading of 40 wt%, Ru loading of 20 wt%) as comparisons. Calculations from the polarization curves show that the mass-specific exchange current of the RhCr NCs / SAC provided in Example 5 is 225 A / mg, which is 23 times that of PtRu / C under alkaline conditions and 110 times that of Pt / C under alkaline conditions. Compared with other existing high-performance hydroxide catalysts, the RhCr NCs / SAC provided in Example 5 of this invention also has a significant advantage in activity, exceeding 10 times the activity of the best current alkaline hydroxide catalysts.
[0155] Figure 9 The performance diagram shows an alkaline membrane fuel cell assembled using RhCr NCs / SAC as the anode and commercial Pt / C as the cathode, as provided in Example 5. A comparative analysis is provided using alkaline membrane fuel cells assembled with the same Pt / C loading (40 wt% Pt) or PtRu / C (40 wt% Pt and 20 wt% Ru) as the anode catalyst. Test results show that with an anode loading of only 0.01 mg... PGM / cm 2 In this case, the alkaline membrane fuel cell based on RhCr NCs / SAC has a yield of 1.86 W / cm². -2 The peak power density is higher than that of PtRu / C (0.58W cm⁻¹) under the same conditions. -2 ) and Pt / C (0.36W cm -2 ).
[0156] Figure 10 yes Figure 9 The peak power density and loading capacity of various fuel cells are compared with those of currently known high-performance alkaline membrane fuel cells. As shown in the figure, compared with other catalytic materials, RhCr NCs / SAC can still maintain high battery performance even with a loading capacity reduction of more than 10 times.
[0157] Figure 11 These are TEM images of composite catalysts formed by metal Rh and single-atom transition metals V, Mn, Fe, Co, Ni, Cu, and Zn modified supports. Figure 11In the figures, a represents a TEM image of the RhV NCs / SAC catalyst provided in Example 6; b represents a TEM image of the RhCr NCs / SAC catalyst provided in Example 5; c represents a TEM image of the RhMn NCs / SAC catalyst provided in Example 7; d represents a TEM image of the RhFe NCs / SAC catalyst provided in Example 8; e represents a TEM image of the RhCo NCs / SAC catalyst provided in Example 9; f represents a TEM image of the RhNi NCs / SAC catalyst provided in Example 10; g represents a TEM image of the RhCu NCs / SAC catalyst provided in Example 11; and h represents a TEM image of the RhZn NCs / SAC catalyst provided in Example 12. As can be seen from the figures, these catalysts all contain 1-2 nm metal clusters and activated carbon supports.
[0158] Figure 12 These are the alkaline hydrogen oxidation polarization curves of the metal Rh / different transition metal single-atom modified carbon support catalysts obtained in Examples 5-12.
[0159] Figure 13 It is based on Figure 12 A comparison of the mass ratio exchange current and corresponding metal nanoparticle activities calculated from the polarization curves of each catalyst is presented. As shown in the figure, the carbon support modified with single atoms of transition metals generally enhances the HOR performance of metal Rh. Under the same loading, RhV NCs / SAC exhibits a 9.35-fold increase in activity compared to Rh / C; RhCrNCs / SAC provided in Example 5 shows a 29.5-fold increase in activity compared to Rh / C; RhMn NCs / SAC shows a 4.79-fold increase in activity compared to Rh / C; RhFeNCs / SAC shows a 2.65-fold increase in activity compared to Rh / C; RhCo NCs / SAC shows an 8.16-fold increase in activity compared to Rh / C; RhNiNCs / SAC shows a 6.26-fold increase in activity compared to Rh / C; RhCu NCs / SAC shows a 6.72-fold increase in activity compared to Rh / C; and RhZnNCs / SAC shows an 8.93-fold increase in activity compared to Rh / C.
[0160] Figure 14 This is a graph showing the electrocatalytic performance of RhCr NCs / SAC. From... Figure 14 As can be seen from the data, under a fixed potential, the catalytic rate of RhCr NCs / SAC did not decrease after 20,000 s, indicating that it has excellent stability.
[0161] Figure 15 The X-ray absorption spectrum of the single-atom Cr-modified carbon support in RhCr NCs / SAC is shown.
[0162] Where a is the X-ray near-edge absorption spectrum, and "Cr foil" is the Cr metal sheet. a shows that the valence state of Cr in the Cr-modified carbon support is +3, which is the same as the valence state of Cr in acetylacetone chromium and chromium trioxide. b is the extended X-ray absorption fine spectrum, which shows the coordination environment of Cr. In the Cr-modified carbon support, Cr is only coordinated with oxygen in the first shell and only Cr-OC bonds exist in the second shell. Therefore, Cr in the Cr-modified carbon support is in a single-atom dispersed state.
[0163] The inventors analyzed the scheme of this invention as follows: The important reason for the enhanced alkaline hydroxide activity of the hydroxide reaction catalysts in Examples 1-5 of this invention is the modification of the noble metal double layer by the single-atom Cr-modified carbon support. Following this method, the inventors synthesized a series of high-performance catalysts. Simultaneously, the inventors also discovered that Cr can be replaced by other elements (Examples 6-12). The inventors provided carbon supports modified with single atoms of 3d transition metals (V, Mn, Fe, Co, Ni, Cu, Zn). The Rh-based catalysts synthesized using these supports also have similar structures, namely, containing Rh nanoclusters and metal single-atom structures. These catalysts also exhibit enhanced alkaline hydroxide activity compared to commercial Rh / C catalysts.
[0164] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A catalyst for a hydrogenation reaction, characterized in that, The catalyst contains a support and a metal active component, wherein the support is a carbon material; the metal active component contains a second metal element and a first metal element; the first metal element is Rh; the second metal element is Cr; and the second metal element is distributed on the carbon material in a single-atom dispersed state. The molar ratio of the second metallic element to the first metallic element is 25:75 to 35:65; Based on the total weight of the carbon material, the loading of the metal active component is 0.5-0.8 wt%; The carbon material is prepared by a method comprising the following steps: (1) At temperature T1, carbon raw material is contacted and mixed with strong acid solution, and the material I obtained after contact mixing is separated to obtain carbon oxide precursor material. T1 is 50-100℃, and the carbon raw material is selected from at least one of carbon black, carbon nanotubes and graphene; the strong acid solution is selected from at least one of nitric acid, sulfuric acid and potassium permanganate. (2) The carbon oxide precursor is dispersed in water and then filtered, and the resulting carbon material is dried to obtain the carbon material.
2. The hydrogenation catalyst according to claim 1, characterized in that, In step (1), the carbon raw material is carbon black and the strong acid solution is nitric acid.
3. The hydrogenation catalyst according to claim 2, characterized in that, The carbon raw material is KB-300J type carbon black; the strong acid solution is an aqueous solution of nitric acid with a concentration greater than 50wt%.
4. The hydrogenation catalyst according to claim 1 or 2, characterized in that, In step (1), before the contact mixing is performed, the carbon raw material and the strong acid solution are first subjected to ultrasonic pretreatment, and then the pretreated mixed solution is subjected to contact mixing.
5. The hydrogenation catalyst according to claim 4, characterized in that, The frequency of the ultrasound is 30kHz-50kHz.
6. The hydrogenation catalyst according to claim 1, characterized in that, The first metal element is distributed on the carrier in the form of metal clusters.
7. The hydrogenation catalyst according to claim 6, characterized in that, The average particle size of the metal clusters is no greater than 2 nm.
8. A method for preparing a catalyst for a hydrogenation reaction, characterized in that, The method includes: S1: In a solution environment, the active metal source and the support are mixed to obtain a catalyst precursor; the support is the carbon material described in claim 1; S2: Reduce the catalyst precursor; The active metal source is selected from substances capable of providing active metal components, wherein the active metal components contain a second metal element and a first metal element, wherein the first metal element is Rh and the second metal element is Cr.
9. The method according to claim 8, characterized in that, In step S1, the conditions for the mixing process include: a temperature of 30-80℃ and a time of 0.1-5h.
10. The method according to claim 9, characterized in that, In step S1, the mixing process is performed under ultrasonic conditions.
11. The method according to claim 10, characterized in that, The frequency of the ultrasound is 30kHz-50kHz.
12. The hydrogenation catalyst prepared by the method according to any one of claims 8-11.
13. The use of the hydroxide reaction catalyst according to any one of claims 1-7 in the alkaline hydrogen oxidation reaction.
Citation Information
Patent Citations
Platinum-carbon catalyst and preparation method and application thereof
CN111146448A
Hydroxidation catalyst with carbon monoxide poisoning resisting function and preparation method thereof