Preparation method and application of highly permeable carbon paper for fuel cells
Through the combination of modified carbon fiber and polytetrafluoroethylene, highly breathable carbon paper is formed, which solves the problem of poor breathability of carbon paper for fuel cells, achieves excellent breathability and conductivity, and improves the efficiency of fuel cells.
Patent Information
- Application Number
- CN202311850669.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-12-29
AI Technical Summary
The breathable performance of carbon paper for fuel cells is not excellent enough, and existing density enhancement methods will damage mechanical properties and conductivity, resulting in a reduction in battery efficiency.
Using a combination of modified carbon fiber and modified polytetrafluoroethylene, the highly breathable carbon paper is formed by sonication, impregnation and curing treatment, and 2,4-diaminodiphenylamine and 2-(benzyloxy)-3 are used. ,5-dichlorobenzoic acid modified carbon fiber, combined with neopentyl borate modified polytetrafluoroethylene, forming a breathable rigid channel from the inside to the outside.
It significantly improves the breathability and conductivity of carbon paper, with a breathability of up to 2500ml*mm/(cm*h*mmAQ), and a resistivity as low as below 9mΩ·cm, improving the material transmission performance of fuel cells.
Smart Images

Figure BDA0004640931110000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a preparation method and application of highly air-permeable carbon paper for fuel cells. Background Art
[0002] Carbon paper is the key supporting material for the gas diffusion layer of proton exchange membrane fuel cells. Its porosity, pore structure and electrical conductivity determine the material transfer performance of carbon paper as the diffusion layer substrate. Insufficient porosity often leads to flooding and mass transfer polarization of the electrode, which reduces the battery efficiency; if the porosity is too high, the density and conductivity of the carbon fiber paper are poor, and the mechanical behavior is insufficient. Although there are various densification methods such as composite resins and adding nanofibers, the resin is a hard carbon phase after carbonization, and the crystallinity is poor, which increases the difficulty of graphitization treatment. It is not only costly, but the internal stress caused by high temperature will also damage the mechanical properties; other nanofibers, plant fibers, etc. have unsatisfactory electrical conductivity, and their addition will damage the conductive properties of carbon fiber paper; these two solutions will also greatly reduce the overall porosity of carbon fiber paper, resulting in a significant decrease in air permeability. To solve the above contradictions, the current effective means are usually to add conductive carbon fillers to the carbon fiber paper blank to achieve the densification of carbon fiber paper and improve the electrical conductivity and mechanical properties at the same time. CN115387148A discloses a high-conductivity, high-air-permeability gradient-structured carbon fiber paper and a preparation method thereof. However, the air permeability of the carbon fiber paper is not excellent enough.
[0003] In summary, after extensive searching by the applicant, it is found that at least in the art, the air permeability of carbon paper for fuel cells is not good enough. Therefore, it is necessary to develop or improve a preparation method and application of highly permeable carbon paper for fuel cells. Summary of the invention
[0004] Based on this, in order to solve the problem that the air permeability of carbon paper for fuel cells is not good enough, the present invention provides a preparation method and application of highly permeable carbon paper for fuel cells. The specific technical scheme is as follows:
[0005] A method for preparing highly permeable carbon paper for a fuel cell comprises the following steps:
[0006] Cleaning carbon fibers of 1 to 5 mm to obtain carbon fiber precursors;
[0007] The carbon fiber precursor is subjected to modification treatment to obtain modified carbon fiber;
[0008] The modified carbon fiber is added into water, ultrasonicated at a frequency of 110 to 130 kHz for 30 to 40 minutes, then a 0.5 to 0.9 wt % hydroxyethyl cellulose aqueous solution is added, stirred evenly at a speed of 1400 to 1500 r / min, and then added into a former for wet forming to obtain a carbon paper base paper;
[0009] The carbon paper base paper is immersed in the modification liquid for 1.8 to 2.4 hours, and then dried at 95 to 105° C. in an argon atmosphere, and then cured and carbonized in an argon atmosphere to obtain the highly permeable carbon paper for the fuel cell;
[0010] The modified liquid includes modified polytetrafluoroethylene, a conductive material and a solvent;
[0011] The raw materials for the modified carbon fiber modification treatment include carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid;
[0012] The raw materials for preparing the modified polytetrafluoroethylene include polytetrafluoroethylene and phenyl boric acid neopentyl glycol ester.
[0013] Furthermore, the modification process comprises the following steps:
[0014] The carbon fiber precursor is added to 25-35wt% nitric acid, stirred evenly at a speed of 900-1000r / min, then heated to 40-45°C for reaction for 2-3h, then filtered and separated, the precipitate is washed and dried, and N,N-dimethylformamide is added, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid are added at a stirring speed of 850-950r / min, and then palladium acetate and manganese chloride are added, and the temperature is raised to 92-98°C for reaction for 18-22h to obtain the modified carbon fiber.
[0015] Furthermore, the cleaning process comprises the following steps:
[0016] The carbon fiber is immersed in a 6-8wt% sodium hydroxide ethanol solution for 8-10 hours, then filtered and separated, washed with ethanol to a pH of 6.5-7.5, then added with 10-15wt% hydrochloric acid, ultrasonicated at a frequency of 50-70kHz for 20-30min, then washed with water to a pH of 6.5-7.5, then heated to 65-75°C and dried to obtain the carbon fiber precursor.
[0017] Furthermore, the preparation method of the modified polytetrafluoroethylene comprises the following steps:
[0018] The polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 70 to 90 kHz for 15 to 25 minutes, then phenyl boric acid neopentyl glycol ester is added, stirred evenly at a speed of 800 to 900 r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 132 to 138° C., reacted for 7 to 9 hours, then acidified, and separated to obtain modified polytetrafluoroethylene.
[0019] Furthermore, the conductive material includes at least one of conductive carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene.
[0020] Furthermore, the solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
[0021] Furthermore, the curing treatment is carried out under the conditions of keeping the temperature at 250-270° C. for 2.2-2.8 hours.
[0022] Furthermore, the carbonization treatment is carried out under the conditions of keeping the temperature at 2200-2300° C. for 1.3-1.7 hours.
[0023] Furthermore, the mass ratio of the carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid is 98-102:3-7:3-7;
[0024] The mass ratio of the polytetrafluoroethylene to the phenyl boric acid neopentyl glycol ester is 98-102:5-10.
[0025] The technical solution also provides a fuel cell, which includes a proton exchange membrane, a gas diffusion layer, a catalyst layer and a bipolar plate, wherein the gas diffusion layer includes carbon paper, and the carbon paper is the highly permeable carbon paper for the fuel cell.
[0026] The preparation method uses modified carbon fibers modified with 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid and modified polytetrafluoroethylene modified with phenylboronic acid neopentyl glycol ester at the same time, so that the prepared carbon paper for fuel cells has excellent air permeability and excellent electrical conductivity. Specifically, concentrated nitric acid can partially nitrate the carbon fibers, and 2-(benzyloxy)-3,5-dichlorobenzoic acid reacts with nitro and 2,4-diaminodiphenylamine at the same time under the catalysis of palladium acetate, so that a large-occupying rigid aromatic group is linked to the surface of the carbon fibers, thereby significantly increasing the air permeability of the modified carbon fibers; further, polytetrafluoroethylene and phenylboronic acid neopentyl glycol ester can undergo an arylation reaction under the catalysis of dodecacarbonyl triruthenium, so that the modified polytetrafluoroethylene is linked with a rigid aromatic group; when the modified polytetrafluoroethylene is impregnated in the modified carbon fibers, an air-permeable rigid channel from the inside to the outside can be effectively formed, thereby significantly improving the air permeability of the prepared carbon paper. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0029] A method for preparing highly permeable carbon paper for a fuel cell in one embodiment of the present invention comprises the following steps:
[0030] Cleaning carbon fibers of 1 to 5 mm to obtain carbon fiber precursors;
[0031] The carbon fiber precursor is subjected to modification treatment to obtain modified carbon fiber;
[0032] The modified carbon fiber is added into water, ultrasonicated at a frequency of 110 to 130 kHz for 30 to 40 minutes, then a 0.5 to 0.9 wt % hydroxyethyl cellulose aqueous solution is added, stirred evenly at a speed of 1400 to 1500 r / min, and then added into a former for wet forming to obtain a carbon paper base paper;
[0033] The carbon paper base paper is immersed in the modification liquid for 1.8 to 2.4 hours, and then dried at 95 to 105° C. in an argon atmosphere, and then cured and carbonized in an argon atmosphere to obtain the highly permeable carbon paper for the fuel cell;
[0034] The modified liquid comprises modified polytetrafluoroethylene, a conductive material and a solvent.
[0035] The raw materials for the modified carbon fiber modification treatment include carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid;
[0036] The raw materials for preparing the modified polytetrafluoroethylene include polytetrafluoroethylene and phenyl boric acid neopentyl glycol ester.
[0037] In one embodiment, the modification process comprises the following steps:
[0038] The carbon fiber precursor is added to 25-35wt% nitric acid, stirred evenly at a speed of 900-1000r / min, then heated to 40-45°C for reaction for 2-3h, then filtered and separated, the precipitate is washed and dried, and N,N-dimethylformamide is added, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid are added at a stirring speed of 850-950r / min, and then palladium acetate and manganese chloride are added, and the temperature is raised to 92-98°C for reaction for 18-22h to obtain the modified carbon fiber.
[0039] In one embodiment, the cleaning process comprises the following steps:
[0040] The carbon fiber is immersed in a 6-8wt% sodium hydroxide ethanol solution for 8-10 hours, then filtered and separated, washed with ethanol to a pH of 6.5-7.5, then added with 10-15wt% hydrochloric acid, ultrasonicated at a frequency of 50-70kHz for 20-30min, then washed with water to a pH of 6.5-7.5, then heated to 65-75°C and dried to obtain the carbon fiber precursor.
[0041] In one embodiment, the method for preparing the modified polytetrafluoroethylene comprises the following steps:
[0042] The polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 70 to 90 kHz for 15 to 25 minutes, then phenyl boric acid neopentyl glycol ester is added, stirred evenly at a speed of 800 to 900 r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 132 to 138° C., reacted for 7 to 9 hours, then acidified, and separated to obtain modified polytetrafluoroethylene.
[0043] In one embodiment, the conductive material includes at least one of conductive carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene.
[0044] In one embodiment, the solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
[0045] In one embodiment, the curing treatment condition is to keep the temperature at 250-270° C. for 2.2-2.8 hours.
[0046] In one of the embodiments, the carbonization treatment is carried out at 2200-2300° C. for 1.3-1.7 hours.
[0047] In one embodiment, the mass ratio of the carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid is 98-102:3-7:3-7;
[0048] The mass ratio of the polytetrafluoroethylene to the phenyl boric acid neopentyl glycol ester is 98-102:5-10.
[0049] In one embodiment, the technical solution provides a fuel cell, which includes a proton exchange membrane, a gas diffusion layer, a catalyst layer and a bipolar plate, wherein the gas diffusion layer includes carbon paper, and the carbon paper is the highly permeable carbon paper for the above-mentioned fuel cell.
[0050] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0051] Embodiment 1:
[0052] Preparation of modified polytetrafluoroethylene: polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 80kHz for 20 minutes, then phenylboronic acid neopentyl glycol ester is added, stirred evenly at a speed of 850r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 135°C for reaction for 8 hours, then acidified, and the modified polytetrafluoroethylene is separated;
[0053] Preparation of modified liquid: conductive carbon black was added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 min, and then modified polytetrafluoroethylene was added, and stirred evenly at a speed of 1050 r / min to obtain modified liquid;
[0054] The 3 mm carbon fiber was immersed in a 7 wt % sodium hydroxide ethanol solution for 9 h, then filtered and separated, washed with ethanol until the pH was 7, then added with 12 wt % hydrochloric acid, ultrasonicated at a frequency of 60 kHz for 25 min, then washed with water until the pH was 7, then heated to 70 ° C and dried to obtain a carbon fiber precursor; the carbon fiber precursor was added to 30 wt % nitric acid, stirred evenly at a speed of 950 r / min, then heated to 42 ° C and reacted for 2.5 h, then filtered and separated, the precipitate was washed and dried, and N, N-dimethylformamide was added, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid were added at a stirring speed of 900 r / min, and then palladium acetate and manganese chloride were added, and the temperature was raised to 95 ° C and reacted for 20 h to obtain Modified carbon fiber; adding the modified carbon fiber into water, ultrasonicating at a frequency of 120kHz for 35 minutes, then adding 0.7wt% hydroxyethyl cellulose aqueous solution, stirring evenly at a speed of 1450r / min, and then adding into a former for wet forming to obtain carbon paper base paper; immersing the carbon paper base paper in the modified liquid for 2.1 hours, then drying at 100°C under an argon atmosphere, then curing treatment at 260°C for 2.5 hours and carbonization treatment at 2250°C for 1.5 hours under an argon atmosphere to obtain highly permeable carbon paper for fuel cells; wherein the mass ratio of carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid is 100:5:5, and the mass ratio of polytetrafluoroethylene and phenylboronic acid neopentyl glycol ester is 100:7.
[0055] Embodiment 2:
[0056] The other parts are the same as those in Example 1, except that the mass ratio of polytetrafluoroethylene to neopentyl glycol phenyl borate is 100:5.
[0057] Embodiment 3:
[0058] The other parts are the same as those in Example 1, except that the mass ratio of polytetrafluoroethylene to neopentyl glycol phenyl borate is 100:10.
[0059] Comparative Example 1:
[0060] Preparation of modified polytetrafluoroethylene: polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 80kHz for 20 minutes, then phenylboronic acid neopentyl glycol ester is added, stirred evenly at a speed of 850r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 135°C for reaction for 8 hours, then acidified, and the modified polytetrafluoroethylene is separated;
[0061] Preparation of modified liquid: conductive carbon black was added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 min, and then modified polytetrafluoroethylene was added, and stirred evenly at a speed of 1050 r / min to obtain modified liquid;
[0062] The 3 mm carbon fiber was immersed in a 7 wt % sodium hydroxide ethanol solution for 9 h, then filtered and separated, washed with ethanol until the pH was 7, then added with 12 wt % hydrochloric acid, ultrasonicated at a frequency of 60 kHz for 25 min, then washed with water until the pH was 7, then heated to 70 ° C and dried to obtain a carbon fiber precursor; the carbon fiber precursor was added to 30 wt % nitric acid, stirred evenly at a speed of 950 r / min, then heated to 42 ° C and reacted for 2.5 h, then filtered and separated, the precipitate was washed and dried, and N, N-dimethylformamide was added, 2-(benzyloxy)-3,5-dichlorobenzoic acid was added at a stirring speed of 900 r / min, and then palladium acetate and manganese chloride were added, and the temperature was raised to 95 ° C and reacted for 20 h to obtain to modified carbon fiber; adding the modified carbon fiber into water, ultrasonicating at a frequency of 120kHz for 35min, then adding 0.7wt% hydroxyethyl cellulose aqueous solution, stirring evenly at a speed of 1450r / min, and then adding into a former for wet forming to obtain carbon paper base paper; immersing the carbon paper base paper in the modified liquid for 2.1h, then drying at 100℃ under an argon atmosphere, and then curing treatment at 260℃ for 2.5h and carbonization treatment at 2250℃ for 1.5h under an argon atmosphere to obtain highly permeable carbon paper for fuel cells; wherein the mass ratio of carbon fiber to 2-(benzyloxy)-3,5-dichlorobenzoic acid is 100:5, and the mass ratio of polytetrafluoroethylene to phenylboronic acid neopentyl glycol ester is 100:7.
[0063] Comparative Example 2:
[0064] Preparation of modified polytetrafluoroethylene: polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 80kHz for 20 minutes, then phenylboronic acid neopentyl glycol ester is added, stirred evenly at a speed of 850r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 135°C for reaction for 8 hours, then acidified, and the modified polytetrafluoroethylene is separated;
[0065] Preparation of modified liquid: conductive carbon black was added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 min, and then modified polytetrafluoroethylene was added, and stirred evenly at a speed of 1050 r / min to obtain modified liquid;
[0066] The 3mm carbon fiber was immersed in a 7wt% sodium hydroxide ethanol solution for 9h, then filtered and separated, washed with ethanol to a pH of 7, then added with 12wt% hydrochloric acid, ultrasonicated at a frequency of 60kHz for 25min, then washed with water to a pH of 7, then heated to 70°C and dried to obtain a carbon fiber precursor; the carbon fiber precursor was added to 30wt% nitric acid, stirred evenly at a speed of 950r / min, then heated to 42°C and reacted for 2.5h, then filtered and separated, the precipitate was washed and dried, and N,N-dimethylformamide was added, 2,4-diaminodiphenylamine was added at a stirring speed of 900r / min, then palladium acetate and manganese chloride were added, and the temperature was raised to 95°C and reacted for 20h to obtain to modified carbon fiber; adding the modified carbon fiber into water, ultrasonicating at a frequency of 120kHz for 35min, then adding 0.7wt% hydroxyethyl cellulose aqueous solution, stirring evenly at a speed of 1450r / min, and then adding into a former for wet forming to obtain carbon paper base paper; immersing the carbon paper base paper in the modified liquid for 2.1h, then drying at 100℃ under an argon atmosphere, and then curing at 260℃ for 2.5h and carbonizing at 2250℃ for 1.5h under an argon atmosphere to obtain highly permeable carbon paper for fuel cells; wherein the mass ratio of carbon fiber to 2,4-diaminodiphenylamine is 100:5, and the mass ratio of polytetrafluoroethylene to phenyl boric acid neopentyl glycol ester is 100:7.
[0067] Comparative Example 3:
[0068] Preparation of impregnation solution: conductive carbon black is added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 minutes, and then polytetrafluoroethylene is added and stirred at a speed of 1050 r / min to obtain an impregnation solution;
[0069] The 3 mm carbon fiber is immersed in a 7 wt % sodium hydroxide ethanol solution for 9 hours, then filtered and separated, washed with ethanol until the pH is 7, then added with 12 wt % hydrochloric acid, ultrasonicated at a frequency of 60 kHz for 25 minutes, then washed with water until the pH is 7, then heated to 70°C and dried to obtain a carbon fiber precursor; the carbon fiber precursor is added to 30 wt % nitric acid, stirred evenly at a speed of 950 r / min, then heated to 42°C for reaction for 2.5 hours, then filtered and separated, the precipitate is washed and dried, and N, N-dimethylformamide is added, 2, 4-diaminodiphenylamine and 2-(benzyloxy)-3, 5-dichlorobenzoic acid are added at a stirring speed of 900 r / min, and then palladium acetate and manganese chloride are added. The temperature is raised to 95°C for reaction for 20 hours to obtain modified carbon fiber; the modified carbon fiber is added into water, ultrasonicated at a frequency of 120kHz for 35 minutes, then a 0.7wt% hydroxyethyl cellulose aqueous solution is added, stirred evenly at a speed of 1450r / min, and then added into a former for wet forming to obtain carbon paper base paper; the carbon paper base paper is immersed in the impregnation liquid for 2.1 hours, then dried at 100°C under an argon atmosphere, then kept at 260°C for 2.5 hours under an argon atmosphere for curing treatment and kept at 2250°C for 1.5 hours for carbonization treatment to obtain highly permeable carbon paper for fuel cells; wherein the mass ratio of carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid is 100:5:5.
[0070] Comparative Example 4:
[0071] Preparation of modified polytetrafluoroethylene: polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 80kHz for 20 minutes, then phenylboronic acid neopentyl glycol ester is added, stirred evenly at a speed of 850r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 135°C for reaction for 8 hours, then acidified, and the modified polytetrafluoroethylene is separated;
[0072] Preparation of modified liquid: conductive carbon black was added to ethanol, ultrasonicated at a frequency of 80 kHz for 35 min, and then modified polytetrafluoroethylene was added, and stirred evenly at a speed of 1050 r / min to obtain modified liquid;
[0073] A 3 mm carbon fiber is immersed in a 7 wt % sodium hydroxide ethanol solution for 9 hours, then filtered and separated, washed with ethanol to a pH of 7, then added with 12 wt % hydrochloric acid, ultrasonicated at a frequency of 60 kHz for 25 minutes, then washed with water to a pH of 7, then heated to 70°C and dried to obtain a carbon fiber precursor; the carbon fiber precursor is added to water, ultrasonicated at a frequency of 120 kHz for 35 minutes, then added with a 0.7 wt % hydroxyethyl cellulose aqueous solution, stirred evenly at a speed of 1450 r / min, and then added to a former for wet molding to obtain a carbon paper base paper; the carbon paper base paper is immersed in a modified liquid for 2.1 hours, then dried at 100°C under an argon atmosphere, then kept at 260°C for 2.5 hours under an argon atmosphere for curing treatment and kept at 2250°C for 1.5 hours for carbonization treatment to obtain a highly permeable carbon paper for fuel cells; wherein the mass ratio of polytetrafluoroethylene to phenyl boric acid neopentyl glycol ester is 100:7.
[0074] The carbon papers obtained in Examples 1 to 3 and Comparative Examples 1 to 4 were tested for air permeability and electrical conductivity. The test results are shown in Table 1.
[0075] Table 1:
[0076]
[0077] As can be seen from Table 1, the preparation methods provided in Examples 1 to 3 use modified carbon fibers modified with 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid and modified polytetrafluoroethylene modified with phenylboronic acid neopentyl glycol ester at the same time, so that the prepared carbon paper for fuel cells has excellent air permeability and excellent electrical conductivity. Specifically, its air permeability is as high as 2500ml*mm / (cm*h*mmAQ) or more, and its resistivity is as low as 9mΩ·cm or less. More specifically, concentrated nitric acid can partially nitrate the carbon fibers, and 2-(benzyloxy)- 3,5-Dichlorobenzoic acid undergoes a coupling reaction with nitro and 2,4-diaminodiphenylamine at the same time under the catalysis of palladium acetate, thereby linking a large-occupying rigid aromatic group on the surface of the carbon fiber, thereby significantly increasing the air permeability of the modified carbon fiber; further, polytetrafluoroethylene and neopentyl glycol phenylboronate can undergo an arylation reaction under the catalysis of triruthenium dodecacarbonyl, thereby linking a rigid aromatic group on the modified polytetrafluoroethylene; when the above-mentioned modified polytetrafluoroethylene is impregnated in the above-mentioned modified carbon fiber, a breathable rigid channel from the inside to the outside can be effectively formed, thereby significantly improving the air permeability of the prepared carbon paper.
[0078] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0079] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing highly permeable carbon paper for fuel cells, characterized in that: It includes the following steps: Cleaning carbon fibers of 1 to 5 mm to obtain carbon fiber precursors; The carbon fiber precursor is subjected to modification treatment to obtain modified carbon fiber; The modified carbon fiber is added into water, ultrasonicated at a frequency of 110 to 130 kHz for 30 to 40 minutes, then a 0.5 to 0.9 wt % hydroxyethyl cellulose aqueous solution is added, stirred evenly at a speed of 1400 to 1500 r / min, and then added into a former for wet forming to obtain a carbon paper base paper; The carbon paper base paper is immersed in the modification liquid for 1.8 to 2.4 hours, and then dried at 95 to 105° C. in an argon atmosphere, and then cured and carbonized in an argon atmosphere to obtain the highly permeable carbon paper for the fuel cell; The modified liquid includes modified polytetrafluoroethylene, a conductive material and a solvent; The raw materials for the modified carbon fiber modification treatment include carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid; The raw materials for preparing the modified polytetrafluoroethylene include polytetrafluoroethylene and phenyl boric acid neopentyl glycol ester; The modification process comprises the following steps: The carbon fiber precursor is added to 25-35wt% nitric acid, stirred evenly at a speed of 900-1000r / min, then heated to 40-45°C for reaction for 2-3h, then filtered and separated, the precipitate is washed and dried, and N,N-dimethylformamide is added, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid are added at a stirring speed of 850-950r / min, and then palladium acetate and manganese chloride are added, and the temperature is raised to 92-98°C for reaction for 18-22h to obtain the modified carbon fiber.
2. The preparation method according to claim 1, characterized in that: The cleaning process comprises the following steps: The carbon fiber is immersed in a 6-8wt% sodium hydroxide ethanol solution for 8-10 hours, then filtered and separated, washed with ethanol to a pH of 6.5-7.5, then added with 10-15wt% hydrochloric acid, ultrasonicated at a frequency of 50-70kHz for 20-30min, then washed with water to a pH of 6.5-7.5, then heated to 65-75°C and dried to obtain the carbon fiber precursor.
3. The preparation method according to claim 1, characterized in that: The preparation method of the modified polytetrafluoroethylene comprises the following steps: The polytetrafluoroethylene is added to toluene, ultrasonicated at a frequency of 70 to 90 kHz for 15 to 25 minutes, then phenyl boric acid neopentyl glycol ester is added, stirred evenly at a speed of 800 to 900 r / min, then triruthenium dodecacarbonyl and potassium carbonate are added, the temperature is raised to 132 to 138° C., reacted for 7 to 9 hours, then acidified, and separated to obtain modified polytetrafluoroethylene.
4. The preparation method according to claim 1, characterized in that: The conductive material includes at least one of carbon nanotubes, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene.
5. The preparation method according to claim 1, characterized in that: The solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
6. The preparation method according to claim 1, characterized in that: The curing treatment is carried out under the conditions of keeping the temperature at 250-270° C. for 2.2-2.8 hours.
7. The preparation method according to claim 1, characterized in that: The carbonization treatment is carried out under the conditions of keeping the temperature at 2200-2300° C. for 1.3-1.7 hours.
8. The preparation method according to claim 1, characterized in that: The mass ratio of the carbon fiber, 2,4-diaminodiphenylamine and 2-(benzyloxy)-3,5-dichlorobenzoic acid is 98-102:3-7:3-7; The mass ratio of the polytetrafluoroethylene to the phenyl boric acid neopentyl glycol ester is 98-102:5-10.
9. A fuel cell comprising a proton exchange membrane, a gas diffusion layer, a catalyst layer and a bipolar plate, wherein the gas diffusion layer comprises carbon paper, characterized in that: The carbon paper is the highly air-permeable carbon paper for fuel cells prepared by the method for preparing highly air-permeable carbon paper for fuel cells according to claim 1.