A cellulose virus-removing composite membrane and its preparation method
By designing a three-layer cellulose composite membrane, including a pre-filtration layer, a separation layer, and a separation layer, the problems of unstable LRV value and reduced flux during top washing of the cellulose composite membrane were solved, achieving high protein yield and high flux.
Patent Information
- Application Number
- CN202311742211.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-18
AI Technical Summary
Existing cellulose composite membranes exhibit unstable LRV values during top washing, leading to inconsistent protein yields, and the protective layer also affects flux.
The cellulose composite membrane adopts a three-layer structure, including a pre-filtration layer, a separation layer, and an isolation layer. The isolation layer is used to protect the separation layer during the preparation process. The pore size and fiber diameter of the isolation layer are designed to be 50-500 nm and 20-120 nm, respectively, and the thickness does not exceed 10 μm, to ensure that the separation layer is not damaged during the top washing process.
This improved the stability of the top wash LRV value of the cellulose composite membrane, ensuring high protein yield while maintaining high flux and mechanical strength.
Smart Images

Figure CN117732274B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of membrane materials technology, and more specifically to a cellulose virus-removing composite membrane and its preparation method. Background Technology
[0002] In biopharmaceuticals, virus removal is a crucial step for several reasons: ① Safety considerations: Since biopharmaceuticals are administered via injection, viral contamination could pose serious health risks. Therefore, ensuring the safety of biopharmaceuticals is paramount. ② Regulatory requirements: Drug regulatory agencies in various countries impose stringent safety requirements on biopharmaceutical products, including the control of viral contamination. Virus removal is essential to meet these requirements during the biopharmaceutical process. ③ Protecting the production process: Viruses can contaminate the production process, leading to production failures or product quality issues. Virus removal protects the production process, ensuring product quality and stability. ④ Ensuring product purity: The presence of viruses can affect product purity and potency. Virus removal ensures that product purity and potency meet expected standards. Therefore, in biopharmaceuticals, virus removal is an indispensable step that ensures product safety, compliance, production process stability, and product quality.
[0003] Currently, the main technology used in the market is membrane separation – utilizing antiviral membranes to efficiently remove viruses, reduce the risk of viral contamination, and improve the safety of biopharmaceutical products. Various materials of antiviral membranes are available on the market; for example, Chinese patent CN1759924A (applied by EMD Millipore) discloses a multilayer composite supercomposite membrane. This composite supercomposite membrane includes at least one first porous membrane layer having a first side and an equivalent second side, and at least one second porous membrane layer having an equivalent first side and a second side. The first and second layers are superimposed and have a porosity transition region from the equivalent first side of the second layer to the equivalent second side of the first layer. At least one of these layers is an asymmetric supercomposite membrane. This composite membrane structure has a strong retention effect on small viruses and can achieve high protein absorption. The efficiency meets the needs of practical applications; however, the following problems exist. First, since this composite membrane is a composite membrane, the pore size will suddenly decrease during the transition from one layer to another. This can easily lead to a large range of particle sizes remaining at the interface of the layers formed by co-casting. This particle loading at the layer boundaries leads to a loss of filter lifespan, i.e., a significant reduction in lifespan. Furthermore, the composite membrane is at risk of delamination / layer separation during pleating. In addition, the film-forming material used to prepare this composite membrane is mainly polyethersulfone. The sulfone group of polyethersulfone has benzene rings on both sides, which makes it less hydrophilic. As a result, the final film will have a certain adsorption effect on proteins, and the protein yield is generally low (proteins are very expensive), reducing economic efficiency.
[0004] To ensure high protein yield and improve economic efficiency, Chinese Patent CN116116247A (application filed by Hangzhou Kebote Filter Material Co., Ltd.) discloses an asymmetric cuprammonium cellulose composite membrane for virus removal and its preparation process. This process employs the cuprammonium method, first dissolving cotton fibers in a cuprammonium solution to form a single-layer casting solution. After pretreatment and phase separation, an asymmetric cellulose composite membrane for virus removal is formed. Because this composite membrane is made of cellulose material, it has strong hydrophilicity and low protein adsorption, resulting in a high protein yield. Simultaneously, this cellulose composite membrane includes a pre-filtration layer for filtering and retaining... The virus separation layer and protective layer consist of a pre-filtration layer with one side as the first outer surface and a protective layer with one side as the second outer surface. Through proper control of the protective layer, it is possible not only to ensure that the separation layer structure of the composite membrane is not easily damaged by mechanical forces, but also to ensure that the introduction of the protective layer structure has a minimal impact on the flux of the composite membrane, allowing it to maintain a high flux. However, this method also has several problems. Firstly, the use of a copper ammonia solution results in significant pollution, making recovery and post-processing difficult. Secondly, this method requires strict control of process parameters. Furthermore, it is highly dangerous and could pose a significant risk to the lives of researchers.
[0005] In virus removal filtration, the presence of a protective layer does indeed help prevent mechanical damage to the membrane's separation layer, thus ensuring efficient membrane retention. However, in practical applications, it has been found that the membrane's separation layer is often not subject to mechanical damage (virus removal membranes are single-use and not recycled, making them less susceptible to damage during use; furthermore, with improved production levels, the likelihood of mechanical damage to the separation layer structure during membrane filter assembly has significantly decreased). Simultaneously, the presence of a protective layer can easily affect the overall membrane flux, as the protective layer is generally not very thin (for example, in the embodiment of patent CN116116247A, the thickness of the protective layer is at least 4 micrometers and up to 17 μm). Since cellulose virus removal membranes generally have low flux, the presence of a protective layer can actually limit their use in some applications. Therefore, in some applications, cellulose virus removal membranes often do not require a protective layer. For example, Chinese patent CN116236925A (applied by Hangzhou Kebote Filter Material Co., Ltd.) discloses an asymmetric regenerated cellulose virus removal composite membrane and its preparation process, which uses a double-layer casting process to form a double-layer membrane through a double-layer casting liquid. A liquid-liquid membrane (with a small molecule alcohol added to the casting solution to facilitate mass transfer between the two liquid layers) is followed by pretreatment and curing processes to obtain a corresponding composite membrane. This composite membrane includes a pre-filtration layer, a pore size transition layer, and a separation layer. The pore size transition layer has a small thickness and a small pore size variation coefficient, which allows the composite membrane to not only have good virus retention but also high flux, loading capacity, and protein yield. These advantages make the cellulose virus-removing membrane widely applicable. However, it is often observed that some composite membranes in a batch show good integrity in the initial integrity test, and their various properties (such as retention performance) are excellent. But in actual use, especially during top washing, the LRV (Liquid Retention Value) decreases significantly, which in turn affects the protein yield. (The separation layer was not mechanically damaged during use, and the membrane was filtered before integrity testing, which still showed good results, proving that the decrease in LRV during top washing was not due to mechanical damage.) This suggests a certain deviation in the consistency of top washing between batches of cellulose virus-removing membranes, thus affecting economic efficiency to some extent.
[0006] In conclusion, the existence of the aforementioned problems has, to some extent, limited the development of antiviral membranes. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the present invention aims to provide a cellulose virus-removing composite membrane and its preparation method. The composite membrane mainly comprises a pre-filtration layer, a separation layer, and an isolation layer for isolating and protecting the separation layer. By setting the isolation layer, the separation layer is isolated and protected during membrane preparation, avoiding various damages to the separation layer that could affect the top wash LRV. The final cellulose virus-removing composite membrane maintains high retention efficiency while still having a top wash LRV greater than 4, indicating high consistency of top wash LRV across membrane batches and ensuring high protein yield. In addition, the composite membrane also has good throughput.
[0008] To achieve the above objectives, the present invention provides the following technical solution: a cellulose virus-removing composite membrane comprising a main body having non-directional tortuous pathways within the main body, one side surface of the main body being a first outer surface, and the other side surface of the main body being a second outer surface; the main body includes a pre-filtering layer, a separation layer for intercepting viruses, and an isolation layer for isolating and protecting the separation layer; the pre-filtering layer is located on the side of the separation layer opposite to the isolation layer; one side of the isolation layer is the second outer surface; the average pore size of the isolation layer is larger than the average pore size of the separation layer; the second outer surface has a plurality of second pores, the SEM average pore size of the second pores being 50–500 nm;
[0009] The isolation layer contains isolation fibers for forming a porous structure, and the average SEM diameter of the isolation fibers is 20–120 nm; the thickness of the isolation layer is not higher than 10 μm.
[0010] The average pore size of the PMI of the composite membrane is 15–30 nm.
[0011] For PP7 bacteriophage, the top wash LRV of the composite membrane is not less than 4.
[0012] In the field of virus removal, the presence of a protective layer helps to prevent mechanical damage to the membrane's separation layer during membrane assembly and / or use, thus ensuring high retention efficiency. However, in practical applications, researchers have found that the membrane's separation layer is often not subject to mechanical damage, and the presence of a protective layer can easily affect the overall flux of the membrane. Therefore, cellulose virus removal membranes often do not require a protective layer in applications. With continuous use, researchers have observed that a portion of composite membranes in a batch often perform well in initial integrity tests, and their various properties (such as retention performance) are also excellent (in which case we consider these composite membranes to meet the shipping standards, capable of efficiently retaining viruses and achieving high protein yields). However, in actual use, the retention efficiency of this part of the composite membrane changed significantly during the top washing process, with the top washing LRV value dropping below 4, which could not meet the needs of practical applications and would also affect the protein yield. However, after filtration, the researchers also conducted corresponding integrity tests, and the integrity test results were still good, indicating that the separation layer of the membrane had not been subjected to any mechanical damage. This showed that the decrease in top washing LRV was not due to mechanical damage to the membrane. At this point, the researchers believed that there was a problem with the consistency of the top washing LRV of this batch of cellulose virus removal membranes. As for why the consistency problem occurred, the researchers have not been able to figure it out. Because they do not know what caused the problem, they have not been able to make targeted improvements.
[0013] Through extensive and continuous research, it was discovered that the problem with top-wash LRV of the same batch of membranes occurred because the casting solution used to form the separation layer was in direct contact with the carrier (release membrane or steel strip). The preferred carrier was the release membrane, which is cleaner and smoother (although it may still contain various small impurities that can damage the separation layer). However, even when using a release membrane as a carrier, the separation layer is easily damaged during the separation process (the separation layer is easily damaged during peeling). These damages are not detected during integrity testing or routine retention testing, but they are detected during top washing. This has a certain impact on the process; this is because in actual interception, the existence of the separation layer is partly for the actual interception effect, while the part of the separation layer near the liquid outlet surface is to ensure a low leakage possibility (except for virus filtration, which is dead-end filtration, the separation layer is generally near the liquid outlet surface). Although it has interception capacity, it does not play a interception role; during the top washing process, after the pressure is removed, some viruses are released due to Brownian motion. If there are certain defects in the area of the separation layer near the liquid outlet surface (the second outer surface of this invention is the liquid outlet surface), then these released viruses are more likely to leak from the corresponding defects during top washing. Since the virus did not move to this location during the integrity and retention tests, the integrity and retention test results were unaffected. However, the impact on the top washing results was significant. Only during top washing could the virus potentially move to the vicinity of the liquid outlet (i.e., the second outer surface) and leak. Having discovered this issue, the applicant implemented a protective isolation layer during the preparation process to prevent damage. This involved using a double-layer or multiple-layer casting solution, with the casting solution used to form the macroporous layer (isolation layer) directly contacting the carrier. This prevented damage to the separation layer, which would affect the top washing LRV, thus ensuring that the top washing LRV of the same batch of membranes was almost identical and could meet the needs of practical applications. The applicant particularly wants to emphasize that the discovery of this technical problem itself is inventive and not obvious to those skilled in the art.
[0014] The composite membrane of this invention is made of cellulose-based materials. Compared with other organic polymer film-forming materials such as PES (polyethersulfone), membranes made of cellulose-based materials have strong hydrophilicity, good biocompatibility, and are non-toxic. They also have low adsorption capacity for various proteins (cellulose-based composite membranes are generally considered to be the least protein-adsorbing membrane materials among organic composite membranes). Therefore, they are particularly suitable for use as virus removal membranes. In this invention, "composite" means that the membrane is made from two or even three layers of casting solution, rather than from a single casting solution. However, the film-forming materials in the multilayer casting solution are all cellulose-based materials.
[0015] The cellulose virus-removing composite membrane structure provided by this invention includes a pre-filtration layer, a separation layer, and an isolation layer. The pre-filtration layer traps large particulate impurities in the fluid, acting as a pre-filter. The separation layer, the smallest pore size region in the membrane structure, efficiently traps various viruses (e.g., mouse parvovirus). The isolation layer protects the separation layer during preparation, preventing damage (peeling damage, impurity damage) and ensuring the membrane maintains a high LRV value during top washing (the top washing LRV of the same batch of membranes is generally similar). Stable and with good uniformity, this is completely different from the existing methods that rely on protective layers to prevent mechanical damage during membrane assembly, transportation, and use. Further research revealed that effectively protecting the membrane pores of the separation layer from various influences during preparation depends primarily on the properties of the isolation layer, with the most critical being the pore size of the second outer surface (i.e., the average pore size of the second pores) and the isolation fibers within the isolation layer. Firstly, the second outer surface (generally the liquid outlet surface) is the area in direct contact with the carrier within the isolation layer and even the entire membrane. When the pore size of the second pores on the second outer surface is too large, then the... The outer surface of the second pore cannot effectively isolate and protect the separation layer; and if the pore size of the second pore is too small, it will affect the overall membrane flux. Research has found that when the SEM average pore size of the second pore is 50–500 nm, the outer surface can provide initial isolation and protection for the separation layer without significantly affecting the overall membrane flux. Inside the separation layer, the isolation fibers provide further protection, thus requiring the isolation fibers to have a certain diameter (the diameter cannot be too small, otherwise it will affect the isolation and protection effect; the diameter cannot be too large, otherwise it will affect the membrane flux). (Quantity); Studies have shown that the average SEM diameter of the isolation fiber is 20-120 nm. Under the action of such a fine isolation fiber, it further plays a role in isolating and protecting the separation layer, avoiding damage to the separation layer during the preparation and peeling process; In this invention, by the combined action of the average SEM pore size of the appropriate second pore and the average SEM diameter of the isolation fiber, the separation layer is isolated and protected, resulting in a high top wash LRV of the membrane (high uniformity of membrane top wash LRV). For PP7 phage, the top wash LRV of the composite membrane is not less than 4; while basically not affecting the flux, the overall flux of the membrane remains high.
[0016] Furthermore, the thickness of the isolation layer in this invention is no more than 10 μm, meaning it is desirable to be relatively thin so that it has little impact on membrane flux. This is completely different from the concept that the protective layer needs to have a certain thickness. This is because the isolation layer in this invention is mainly used to protect the separation layer during the preparation and peeling process, while conventional protective layers are used to protect the separation layer from mechanical damage during the transportation and use of the membrane module.
[0017] The average pore size of the composite membrane was tested using a PMI pore size analyzer, and the average PMI pore size of the composite membrane of the present invention was found to be 15-30 nm. Furthermore, the tortuous pathways of the main structure and the certain thickness of the membrane ensure that the composite membrane has a strong retention effect on nanoscale small viruses (even mouse parvovirus with a particle size of 20 nm), which can meet the needs of practical applications and is suitable for use as a virus membrane.
[0018] In this invention, the non-directional tortuous pathway refers to a randomly oriented groove structure and / or a discretely distributed pore structure, and each non-directional tortuous pathway is interconnected, thereby improving the filtration accuracy of the composite membrane and ensuring that the composite membrane also has a high interception effect on small viruses.
[0019] To achieve higher protein yields, whether in laboratory validation or actual production processes in biopharmaceutical companies, a top-wash operation (typically at 30 psi) is generally required after virus filtration using a membrane filter (or porous membrane). This is because some protein remains trapped in the porous membrane during virus filtration, and since proteins are very expensive, a top-wash operation is necessary to remove them from the membrane to further improve protein yield. Taking laboratory validation as an example (although the actual production process may differ, the mechanism is the same and can be characterized through laboratory validation), the top-wash operation typically occurs during continuous filtration. When the flux of the membrane filter (or porous membrane) drops to 25% or only a small amount of feed remains, the external pressure is removed and the process is paused for a period of time (e.g., 5 to 15 minutes) to release the protein from the pore structure. Subsequently, a liquid such as a buffer solution is added to elute the released protein from the porous membrane, thereby improving protein yield.
[0020] The composite membrane of this application includes a pre-filtration layer, a separation layer, and an isolation layer. One side of the isolation layer is the second outer surface (generally also the liquid outlet surface), and the average pore size of the isolation layer is larger than that of the separation layer. In this invention, the separation layer also has a basically symmetrical structure, meaning that the membrane pore size within the separation layer does not change significantly with membrane thickness. Therefore, the separation layer and isolation layer in this invention can be divided as follows: After characterizing the membrane cross-section using a scanning electron microscope (SEM) to obtain the corresponding SEM image, starting from the second outer surface of the membrane (generally the liquid outlet surface), draw several straight lines perpendicular to the membrane thickness direction along the membrane cross-section (the spacing between adjacent lines can be 1 μm, 3 μm, 5 μm, or 10 μm, depending on the specific spacing). (Depending on the actual situation), taking one of the straight lines as an example, measure the distance between every two adjacent solid parts of the line. This distance is the pore size of the pore structure between the two adjacent solid parts. Take the arithmetic mean of all pore sizes. This arithmetic mean, to some extent, characterizes the average pore size of the membrane on the horizontal plane where the line is located. The smaller the arithmetic mean, the smaller the membrane pore size on the horizontal plane. If the average pore size represented by two adjacent straight lines is close to the same (the difference in pore size is less than 10 nm), then we consider that these two adjacent straight lines should be located within the separation layer. Then, the distance between the one of these two straight lines closer to the second outer surface and the second outer surface is the thickness of the isolation layer, and this area is the isolation layer.
[0021] The average pore size of a membrane surface can be measured by characterizing the membrane structure using a scanning electron microscope (SEM), followed by measurement using computer software (such as Matlab, NIS-Elements, etc.) or manually, and then performing corresponding calculations. During membrane fabrication, in the direction perpendicular to the membrane thickness (if the membrane is a flat sheet, this direction is planar; if the membrane is a hollow fiber membrane, this direction is perpendicular to the radius), its characteristics, such as pore size distribution, are roughly uniform and consistent. Therefore, the average pore size of a certain area on the corresponding plane can reflect the overall average pore size on that plane. In actual measurement, the membrane surface can be characterized using an electron microscope to obtain the corresponding SEM image. Since the pores on the membrane surface are roughly uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm by 5μm), the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to determine the diameter of all holes on this area, and then calculate to obtain the average pore diameter of the surface. Of course, those skilled in the art can also obtain the above parameters through other measurement methods. The above measurement methods are for reference only.
[0022] As a further improvement of the present invention, the thickness of the isolation layer is 0.2 to 5 μm, preferably 0.5 to 3 μm; the thickness of the isolation layer does not exceed 15% of the overall thickness of the membrane; and the porosity of the isolation layer is not less than 20%.
[0023] In this invention, the role of the isolation layer is to protect the separation layer during the membrane preparation and peeling process, preventing damage to the separation layer (impurity damage and peeling damage). This is unrelated to mechanical damage; therefore, the isolation layer should be as thin as possible, typically 0.2–5 μm, preferably 0.5–3 μm. At this absolute thickness, the isolation layer can both protect the separation layer, ensuring a high LRV value for the membrane during top washing (the separation layer is crucial to the top washing LRV value), and minimize its impact on membrane flux, ensuring a high overall membrane flux. Besides considering the absolute thickness of the isolation layer, the researchers also consider its relative thickness. Research has shown that the thickness of the isolation layer preferably does not exceed 15% of the overall membrane thickness, meaning the isolation layer occupies only a small portion of the main membrane area, further ensuring membrane flux. Furthermore, the porosity within the isolation layer is not less than 20%, further ensuring that fluid can pass through the isolation layer quickly, allowing the overall membrane to still maintain a high flux.
[0024] As a further improvement of the present invention, the area ratio of the pores on the second outer surface is 3% to 40%; some adjacent second pores are separated by surface fibers, and the SEM average width of the surface fibers is 15 to 100 nm.
[0025] A certain number of pores with a certain diameter exist on the second outer surface of the membrane. If the number of pores is too small, it will affect the overall membrane flux; however, if the number of pores is too large, it will affect the pressure resistance of the second outer surface and the overall mechanical strength of the membrane, as well as its isolation and protection effect on the separation layer. Studies have found that when the pore area ratio (the ratio of the sum of the pore areas to the membrane area) of the pores on the second outer surface is 3% to 40%, combined with an appropriate pore diameter, it ensures that the overall membrane still has a high flux and also provides protection for the separation layer. The membrane provides excellent isolation and protection, and also gives the second outer surface good pressure resistance, resulting in high mechanical strength. Furthermore, researchers discovered that because the pore size of the second pores is relatively large to ensure a high overall membrane flux, some second pores may collapse, affecting the membrane's lifespan. Therefore, surface fibers are placed between some adjacent second pores. These surface fibers effectively support the second pores, ensuring the membrane has a good lifespan. Surprisingly, the presence of surface fibers further enhances the isolation and protection of the separation layer, further resolving the issue of consistency in membrane top-wash LRV.
[0026] Furthermore, researchers have discovered that the factors affecting the flux of composite membranes are not only the internal resistance (various structures inside the membrane) but also the external resistance. External resistance refers to the resistance to feed liquid flow caused by external factors, such as the shielding of the membrane pore structure by the component's support structure, which increases the resistance to feed liquid flow. For example, when one side of the separation layer is the liquid outlet, if some of the pore structures on the liquid outlet surface of the composite membrane are shielded, the number of effective pore structures for feed liquid flow on the liquid outlet surface will be significantly reduced. In this case, the external resistance of the composite membrane will increase significantly, and the flux of the composite membrane will also decrease significantly. In this invention, the introduction of an isolation layer with a larger pore size than the separation layer will, admittedly, increase the thickness of the composite membrane and lengthen the tortuous path inside the filter membrane, leading to an increase in the internal resistance of the composite membrane. However, after the introduction of the isolation layer into the composite membrane of this application, when the second outer surface of the composite membrane (i.e., the liquid outlet surface) has a suitable pore size and a suitable number of second pores, the external resistance of the membrane is greatly reduced, thereby further enabling the composite membrane to have a large flux in actual use, which is unexpected and thus further demonstrates its inventiveness.
[0027] The method for testing the porosity can involve characterizing the membrane structure using a scanning electron microscope, followed by measurement and calculation using computer software (such as Matlab, NIS-Elements, etc.) or manually; a specific area is selected, for example, 1 μm. 2 (1μm x 1μm) or 25μm 2 (5μm multiplied by 5μm), the specific area size depends on the actual situation. Then, use appropriate computer software or manual measurement to find the area of all holes on this area, then calculate and sum them, and then divide by the corresponding area to obtain the porosity of the surface. Of course, those skilled in the art can also obtain the above parameters through other measurement methods. The above measurement methods are for reference only. In addition, the average width of surface fibers by SEM can also be obtained by a similar method (i.e., the average width of several surface fibers on a certain area).
[0028] As a further improvement of the present invention, the pore size variation coefficient S of the isolation layer (0.9~1) / (0~0.1) Not less than 3, preferably not less than 5;
[0029] The area of the isolation layer closest to the first outer surface is considered as 0, and the area of the second outer surface is considered as 1.
[0030]
[0031] In a multilayer composite supercomposite membrane disclosed in patent CN1759924A, abrupt changes between layers are undesirable, meaning that large variations in pore size between adjacent layers are undesirable (abrupt pore size changes easily lead to a large range of particle sizes remaining at the interface of layers formed through co-casting, and this particle loading at the layer boundaries leads to a loss of filter lifespan). In a virus-removing composite membrane disclosed in patent CN116236925A, a gradual change in pore size transition layer is desired. When the thickness of the pore size transition layer is small and the pore size change coefficient is small, it is less likely to cause concentrated retention and lead to local blockage and rapid flux decay due to abrupt pore size changes, thus having a larger loading capacity. Therefore, those skilled in the art would generally consider that a gradual change in pore size between layers is preferred, rather than an abrupt change; however, this invention… However, it is desirable that the pore size between the separation layer and the isolation layer changes abruptly (significantly). This is because, in this invention, the separation layer is used to effectively trap viruses. To ensure trapping efficiency, the pore size of its internal membrane must be very small, and it is also the region with the smallest pore size inside the membrane. On the other hand, the main function of the isolation layer is to isolate and protect the separation layer during the membrane preparation and peeling process. Therefore, the pore size of its internal membrane is desired to be larger (even very large) to reduce the impact on the overall membrane flux (i.e., similar to the membrane flux without the isolation layer). This requires a significant, even abrupt, change in pore size from the separation layer to the isolation layer. This is completely different from the existing understanding of those skilled in the art, meaning that this invention overcomes the corresponding technical bias and is inventive.
[0032] Since the composite membrane in this invention is prepared by multilayer casting solution, and the film-forming substances in the multilayer casting solution are all cellulose polymers, there will inevitably be some mass transfer between adjacent casting solution layers. However, we only want a slight mass transfer to create a sudden change. Due to the mass transfer, the pore size of the pores on the side of the isolation layer near the separation layer will not differ significantly from the pore size of the membrane pores in the separation layer. However, when there is no mass transfer, the pore size of the membrane pores in the isolation layer will change rapidly, resulting in a larger pore size change on the side of the isolation layer near the second outer surface than on the side near the first outer surface. Furthermore, in this invention, a pore size change coefficient S is used... (0.9~1) / (0~0.1) The value is used to characterize the overall pore size change of the isolation layer. The larger the value, the greater the abrupt change in membrane pore size between the isolation layer and the separation layer. Those skilled in the art generally prefer this value to be as small as possible. In this invention, the value is not less than 3, preferably not less than 5, which indicates that the pore size of the membrane pores inside the isolation layer has changed significantly with the thickness. This is considered to be an "abrupt change" in the pore size between the separation layer and the isolation layer. This allows the separation layer to have a suitable pore size, such as for efficient virus capture, while basically not affecting the overall membrane flux, thus truly achieving a balance between retention efficiency and flux.
[0033] The pore size variation coefficient of the isolation layer refers to dividing the isolation layer region into 10 equal parts according to its thickness, where the side of the isolation layer closest to the first outer surface is considered to have a film thickness of 0, and the second outer surface is considered to have a film thickness of 1; the pore size of several holes in each region is measured according to actual needs, and then the average value is taken, which is the average pore size of the region.
[0034] As a further improvement of the present invention, the pore size variation coefficient S of the isolation layer (0.4~0.5) / (0~0.1) The value is 1.1 to 2; and / or, the pore size variation coefficient S of the isolation layer is... (0.9~1) / (0.5~0.6) The value is 3 to 20, preferably 4 to 10.
[0035] In this invention, to ensure good membrane flux, a "sudden change" in pore size between the separation layer and the isolation layer is desired, i.e., a significant change in membrane pore size. However, due to mass transfer between adjacent casting solutions during preparation, the pore size does not change significantly with thickness within a certain region of the isolation layer (the region of the isolation layer closer to the separation layer). Through adjustment, the pore size variation coefficient S of the isolation layer is... (0.4~0.5) / (0~0.1) The value is 1.1 to 2, which indicates that the pore size does change to some extent with the thickness, but it is not excessively large. This is more conducive to ensuring the overall mechanical strength of the membrane (separation will also occur between layers), so that the composite membrane can perform stable filtration under certain pressure.
[0036] In the region of the isolation layer near the second outer surface, we desire a significant change (i.e., abrupt change) in the membrane pore size with thickness. This is achieved through adjustment, where the pore size variation coefficient S of the isolation layer is... (0.9~1) / (0.5~0.6) The flux is 3 to 20, preferably 4 to 10. This ensures that the overall flux of the membrane will not decrease significantly due to the presence of the isolation layer. In other words, the membrane still has a good flux and can filter various fluids relatively quickly.
[0037] As a further improvement of the present invention, the pore size variation coefficient S of the isolation layer (0.4~0.5) / (0~0.1) The pore size variation coefficient S of the isolation layer (0.9~1) / (0.5~0.6) The ratio of the two is 1:1.5 to 8.
[0038] By adopting the above technical solution, although we hope that the pore size in the isolation layer is much larger than that in the separation layer, the variation of the pore size with thickness in the isolation layer should also be relatively reasonable. If the variation is too slow, the membrane cannot achieve high flux; if the variation is too fast, defects are easily generated inside the isolation layer, which may affect the normal use of the composite membrane. Further research has found that the optimal pore size variation coefficient S of the isolation layer is... (0.4~0.5) / (0~0.1) The pore size variation coefficient S of the isolation layer (0.9~1) / (0.5~0.6)The ratio of the two is 1:1.5 to 8. At this time, the pore size inside the isolation layer changes with the thickness, which ensures the overall flux of the membrane on the one hand, and the overall mechanical strength of the membrane on the other.
[0039] As a further improvement of the present invention, the separation layer has a basically symmetrical structure; the separation layer contains retained fibers for forming a porous structure, and the SEM average diameter of the retained fibers is 15-100 nm;
[0040] The ratio of the average SEM diameter of the isolation fiber to the average SEM diameter of the retained fiber is 1.05 to 3:1.
[0041] By adopting the above technical solution, the separation layer in this invention has a basically symmetrical structure, meaning that the pore size of the membrane pores inside the separation layer does not change significantly with the membrane thickness. This is beneficial for ensuring sufficient retention of various small viruses and also for ensuring a high top-wash LRV, further guaranteeing good consistency of the membrane's top-wash LRV. The retained fibers are used to ensure the stability of the membrane pores within the separation layer. If the retained fibers are too fine, it may affect the stability of the membrane pores within the separation layer and the overall porosity of the membrane; if the retained fibers are too coarse, it may affect the overall flux of the membrane. Research shows that the average SEM diameter of the retained fibers is 15–100 nm, which ensures both... This design ensures the stability of the membrane pores within the separation layer, enabling long-term and efficient virus retention while maintaining a high overall membrane flux. Preferably, the ratio of the average SEM diameter of the isolation fiber to the average SEM diameter of the retention fiber is 1.05 to 3:1, meaning the isolation fiber is slightly thicker than the retention fiber. This allows the isolation fiber to effectively protect the membrane pores within the separation layer, ensuring a good LRV (Large-to-Volume Value) during top washing (the top washing LRV of membranes from the same batch is basically the same, indicating good consistency). Furthermore, the combined effect of the isolation and retention fibers of this thickness ensures high overall mechanical strength of the membrane, facilitating various processing methods for the membrane.
[0042] As a further improvement of the present invention, the average SEM pore size of the separation layer is 25-80 nm, and the ratio of the average SEM pore size of the isolation layer to the average SEM pore size of the separation layer is not less than 3.
[0043] By adopting the above technical solution, the separation layer has a suitable pore size, which can fully capture various small viruses such as PP7 and ensure that the virus will not be leaked. At the same time, through research, it is preferred that the ratio of the average SEM pore size of the isolation layer to the average SEM pore size of the separation layer is not less than 3, that is, the pore size of the two regions has changed significantly (which can be regarded as a mutation). This allows the isolation layer to protect the separation layer on the one hand, and to give the membrane as a whole a high flux on the other hand, enabling it to filter fluids quickly in a short time and achieve a high protein yield.
[0044] As a further improvement of the present invention, the thickness of the separation layer is 15 to 60 μm; the ratio of the thickness of the isolation layer to the thickness of the separation layer is 1:10 to 40.
[0045] By adopting the above technical solution, in addition to the pore size of the separation layer, the thickness of the separation layer also affects the retention efficiency to a certain extent. In this invention, the main body has a non-directional tortuous pathway, which refers to a randomly oriented groove structure and / or a discretely distributed pore structure. The non-directional tortuous pathways are interconnected. Under the combined effect of a suitable separation layer thickness and tortuous pathways, the retention of various small viruses is further guaranteed. At the same time, the isolation layer and the separation layer have a suitable thickness ratio, which is more conducive to the membrane having a high flux. It is also conducive to the isolation layer fully protecting the separation layer, avoiding various damages during the membrane preparation process as much as possible, and further ensuring that the membrane has a high top wash LRV and good uniformity.
[0046] As a further improvement of the present invention, the average pore size of the pre-filter layer is larger than the average pore size of the isolation layer; the pre-filter layer has pre-filter fibers for forming a porous structure, and the SEM average diameter of the pre-filter fibers is 30-150 nm; the ratio of the SEM average diameter of the pre-filter fibers to the SEM average diameter of the isolation fibers is 1.1-4.
[0047] By adopting the above technical solution, the pores in the pre-filtration layer have a larger diameter and higher porosity. This ensures that the composite membrane has a high flow rate and can effectively intercept large particulate impurities (large-diameter viruses) without affecting the subsequent retention of small viruses, resulting in a high dirt-holding capacity and long service life for the composite membrane. Research has found that when the SEM average diameter of the pre-filtration fibers is 30–150 nm, this fiber thickness ensures strong stability of the pores inside the pre-filtration layer, making it less prone to collapse or shrinkage, thus ensuring stable fluid flux. Ultimately, this ensures that the membrane as a whole has high mechanical strength and filtration stability, enabling long-term and efficient virus removal. Furthermore, the ratio of the SEM average diameter of the pre-filtration fibers to that of the isolation fibers is 1.1–4, meaning the pre-filtration fibers are slightly thicker than the isolation fibers. This ratio is beneficial for both high overall membrane flux and high mechanical strength, making the membrane suitable for various processing methods. The thickness of the fiber cross section can be considered as the diameter of the fiber. The average diameter of the pre-filtered fiber in this invention can be calculated by using a scanning electron microscope to characterize the morphology of the composite membrane cross section structure, and then using computer software (such as Matlab, NIS-Elements, etc.) or manual measurement to calculate the average value. Of course, it is understood that those skilled in the art can also obtain the above parameters through other measurement methods.
[0048] As a further improvement of the present invention, one side of the pre-filter layer is a first outer surface, the SEM average pore size of the first outer surface is 200-4000 nm, and the pore area ratio of the first outer surface is 5%-45%.
[0049] By adopting the above technical solution, when the composite membrane of the present invention has only a three-layer structure, that is, when the membrane body includes a pre-filtration layer, a separation layer, and an isolation layer, one side of the pre-filtration layer is the first outer surface, which is also often used as the liquid inlet surface. At this time, there are a certain number of first pores with a certain pore size on the first outer surface of the membrane. As is well known, the pore size and number of membrane pores have a significant impact on the flux and other properties of the membrane. Through research, it is preferred that the SEM average pore size of the first outer surface is 200-4000 nm, and the pore area ratio of the first outer surface is 5%-45%. Through the combined action of the first pores with a certain pore size and the first outer surface with a corresponding pore area ratio, the composite membrane has a large flux, which facilitates the rapid passage of fluid through the composite membrane and shortens the filtration time. At the same time, the first outer surface also has good pressure resistance, ensuring the stability of filtration.
[0050] As a further improvement of the present invention, the main body further includes a microporous membrane support layer, one side of which is a first outer surface, the thickness of which is not less than 50 μm, and the porosity of which is 30% to 70%; the microporous membrane support layer has supporting fibers for forming a porous structure, and the SEM average diameter of which is not less than 50 nm.
[0051] By adopting the above technical solution, in order to improve the pressure resistance of cellulose composite membranes, a support membrane layer with high pressure resistance is often introduced on the basis of the cellulose layer to form a composite membrane structure. The support membrane layer is often a microporous membrane formed by polymer materials. The film-forming material of the microporous membrane support layer is at least one of PVDF, PES, PTFE, Nylon, cellulose, and polyolefin. Optionally, the polyolefin is UPE or PP. The presence of the microporous membrane support layer greatly improves the inherent defect of the relatively soft texture of cellulose film-forming materials. For virus removal filtration processes that use pressure as the filtration driving force, this means that the filtration efficiency can be improved by further increasing the filtration pressure, thereby reducing production costs, which has a very positive effect. Studies have shown that the porosity of the microporous membrane support layer is preferably 30% to 70%. The microporous membrane support layer contains supporting fibers for forming a porous structure. The SEM average diameter of the supporting fibers is not less than 50 nm. Such a microporous membrane support layer is more conducive to enabling the composite membrane to have high flux while having high pressure resistance.
[0052] As a further improvement of the present invention, the thickness of the composite membrane is 50–300 μm, and the porosity is 20%–55%; the flux of the composite membrane is 45–150 L*h. -1 *m -2 @30psi; the composite membrane has an LRV of not less than 4 for PP7 phage; the protein yield of the composite membrane is not less than 98%.
[0053] By adopting the above technical solution, the membrane thickness can be obtained by characterizing the membrane structure using a scanning electron microscope, and then calculating it using computer software (such as Matlab, NIS-Elements, etc.) or by manual measurement. Of course, those skilled in the art can also obtain the above parameters using other measurement methods (such as freeze-drying first, and then measuring with measuring tools). The above measurement methods are for reference only. Since the cellulose membrane shrinks when dry, the thickness of the composite membrane in this invention refers to the thickness in the wet state (the thickness when shrunken). The actual measurement can be performed using a thickness gauge in the wet state, or freeze-drying can be performed first to avoid shrinkage of the composite membrane, and then testing with appropriate tools. When the membrane thickness is too small, its mechanical strength will be low. At the same time, due to the short filtration time, effective filtration cannot be achieved. When the membrane thickness is too large, the filtration time will be too long, and the time cost will be too high. The thickness of the cellulose filter membrane of this invention is 50-300 μm, which ensures that the composite membrane not only has high mechanical strength, but also can achieve effective filtration with high filtration efficiency, short filtration time, and low time cost.
[0054] When the membrane porosity is too high, it leads to low tensile strength, poor mechanical properties, and low industrial practical value, failing to meet market demands. Conversely, when the membrane porosity is too low, it affects the membrane flow rate, resulting in slower filtration speed, longer filtration time, and higher time costs. Furthermore, it results in low dirt-holding capacity, a short service life, and frequent membrane replacements, significantly increasing economic costs. Therefore, a suitable porosity is crucial for the filter membrane, and this porosity is closely related to the composite membrane material. The filter membrane of this invention is made of cellulose-based materials, with a porosity of 20%–55%. This porosity, combined with the membrane material, results in a membrane that not only possesses good tensile strength but also a fast filtration speed, high flow rate, and high dirt-holding capacity, capable of trapping a large number of impurity particles, long service life, and low economic cost.
[0055] Permeation flux, also known as permeation rate or simply flux, refers to the amount of substance that passes through a unit membrane area per unit time under a certain operating pressure during the separation process of a composite membrane. The magnitude of the flux reflects the speed of filtration; the higher the flux, the faster the membrane's filtration speed. In this invention, the flux of the composite membrane is 45–150 L / h.~1 *m ~2 @30psi indicates a relatively high flux, suggesting that the composite membrane has a fast filtration speed. While ensuring retention efficiency, the fluid can pass through the composite membrane quickly, resulting in lower time costs and higher economic benefits.
[0056] The viruses intercepted in this invention are mainly targeted at various viruses with a particle size of 20 nm and above (such as mouse parvovirus, whose particle size is about 20 nm). Using PP7 as a representative virus, interception tests were conducted. The results showed that the LRV of PP7 bacteriophage in the composite membrane of this invention was not less than 4, indicating that the composite membrane has a very high virus interception rate and sufficient retention of viral impurities, meeting the needs of practical applications. Furthermore, the protein yield of the composite membrane is not less than 98%, indicating that the effective protein substance in the fluid is not easily adsorbed onto the membrane. On the one hand, it will not clog the membrane pores, ensuring that the composite membrane still has a high service life; on the other hand, it ensures that the content of the effective protein substance in the fluid changes very little, with minimal protein loss, guaranteeing economic benefits. For the testing method of viral impurities, please refer to patents CN105980037B – Virus Removal Membrane, CN101816898B – Supercomposite Membrane and its Preparation Method, CN1759924B – Supercomposite Membrane and its Preparation Method, etc.
[0057] On the other hand, the present invention also provides a method for preparing a cellulose virus-removing composite membrane, comprising the following steps:
[0058] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; the temperature of the carrier is 2-10°C lower than the temperature of the first casting solution.
[0059] The first casting solution comprises the following raw materials in parts by weight: 10-20 parts of the first film-forming polymer, 50-200 parts of the first organic solvent, and 20-60 parts of the first pore-forming agent;
[0060] The second casting solution comprises the following raw materials in parts by weight: 10-30 parts of the second film-forming polymer, 30-80 parts of the second organic solvent, and 20-40 parts of the second pore-forming agent;
[0061] Both the first film-forming polymer and the second film-forming polymer are cellulose polymers; the viscosity ratio of the first casting solution to the viscosity ratio of the second casting solution is 1:(2-6);
[0062] S2: The bilayer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 2-10s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 20%-40%; the good solvent is at least one selected from acetone, dioxane, dimethylacetamide, N-methylpyrrolidone, acetic acid, propionic acid, butyric acid and valeric acid, and the non-solvent is water or ethanol;
[0063] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 20-60 seconds to obtain a green film. The coagulation bath is water.
[0064] S4. The film-forming agent is placed in an aqueous sodium hydroxide solution for hydrolysis, followed by washing to form a film. As a further improvement of the present invention, the temperature of the first casting solution and the second casting solution is 15-40°C; the viscosity of the first casting solution is 3000-8000 mPa·s; the viscosity of the second casting solution is 10000-30000 mPa·s; the first organic solvent and the second organic solvent are at least one of acetone, dioxane, dimethylacetamide, N-methylpyrrolidone, acetic acid, propionic acid, butyric acid, and valeric acid; the first pore-forming agent is at least one of polyvinylpyrrolidone, polyvinyl alcohol, polyethylene glycol, and polypropylene glycol; the second pore-forming agent is any one of formamide, ethanol, 1-propanol, isopropanol, n-butanol, 1-pentanol, 2-pentanol, and diethylamine.
[0065] As a further improvement of the present invention, a microporous membrane support layer is covered on the double liquid film formed in S1, wherein the film-forming material of the microporous membrane support layer is at least one of PVDF, PES, PTFE, nylon, cellulose and polyolefin; wherein the polyolefin is UPE or PP.
[0066] As a further improvement of the present invention, the temperature of the pre-phase separation liquid is 2 to 15°C higher than the temperature of the second casting liquid; the temperature of the coagulation bath is 15 to 45°C.
[0067] As a further improvement of the present invention, the film obtained by S4 is subjected to crosslinking treatment in a crosslinking agent. After the crosslinking treatment is completed and the film is cleaned, a composite film is obtained. The crosslinking agent is at least one of haloepoxide, dihaloalkanes and dihaloalcohols.
[0068] In preparing the cellulose virus-removing composite membrane of the present invention, a first casting solution and a second casting solution are first prepared. Both the first and second casting solutions are cellulose solutions, each comprising a film-forming polymer, an organic solvent, and a pore-forming agent. The film-forming polymer is a cellulose polymer, preferably one or more of cellulose diacetate, cellulose triacetate, cellulose propionate, cellulose acetate phthalate, cellulose acetate butyrate, and cellulose acetate propionate. These cellulose polymers are readily soluble in their respective organic solvents and possess excellent film-forming and fiber-forming properties. The resulting membrane exhibits strong hydrophilicity and does not readily adsorb effective substances (mainly proteins) from the fluid. The presence of the organic solvent (the first and second organic solvents are both at least one of acetone, dioxane, dimethylacetamide, N-methylpyrrolidone, acetic acid, propionic acid, butyric acid, and valeric acid) further contributes to the membrane's effectiveness. The organic solvent is used to fully dissolve the corresponding cellulose polymers. During phase separation, the organic solvent is dissolved in the coagulation bath, causing the cellulose polymers to precipitate and form a composite membrane with a certain pore size. In addition, a pore-forming agent is added to the casting solution. The first pore-forming agent is at least one of polyvinylpyrrolidone, polyvinyl alcohol, polyethylene glycol, and polypropylene glycol. The second pore-forming agent is any one of formamide, ethanol, 1-propanol, isopropanol, n-butanol, 1-pentanol, 2-pentanol, and diethylamine. The addition of the first pore-forming agent helps to increase the porosity of the isolation layer, thereby increasing the porosity of the composite membrane and reducing the impact of the isolation layer on the overall membrane flux. The presence of the second pore-forming agent helps the membrane to have good overall retention efficiency. With the combined effect of such a two-layer casting solution system and appropriate pre-phase separation and phase separation curing processes, it is possible to obtain a composite membrane with ideal pore size and pore structure. An ideal casting solution formulation has a significant impact on the structure and properties of the final composite membrane, such as affecting the pore size and porosity. A reasonable casting solution formulation ensures that the final composite membrane has ideal pore size and structure. In addition, the temperature of the first and second casting solutions is 15–40°C. The temperatures of the two casting solutions can be the same or different, but the same is preferred.
[0069] According to the formula, ideal first and second casting solutions are prepared. The first casting solution is a dilute solution with a low solid content and relatively low viscosity, used to form an isolation layer; while the second casting solution is a concentrated solution with a relatively high solid content and relatively high viscosity (in addition, the applicant would like to explain that sometimes, in order to further increase the thickness of the pre-filtration layer and improve the overall dirt-holding capacity of the membrane, a layer of dilute solution with a relatively low solid content can be cast on the second casting solution to form a three-layer liquid film); the researchers control the viscosity of the two casting solutions, preferably controlling the viscosity ratio of the first casting solution to the second casting solution to be 1:(2-6), and preferably the viscosity of the first casting solution is 3000-8000 mPa·s and the viscosity of the second casting solution is 10000-30000 mPa·s. Under such viscosity control, the two casting solutions easily form the membrane pore structure required by this invention, while minimizing mass transfer between the two casting solutions, thus preventing significant changes in the pore size between the separation layer and the isolation layer. After preparing the first and second casting solutions, they are sequentially cast onto a carrier to form a double-layer liquid film (i.e., the first casting solution is in direct contact with the carrier; the second casting solution is applied to the first casting solution without contacting the carrier, avoiding various damages to the separation layer during the preparation and peeling process). It should be noted that the casting solution of this invention can be cast manually (e.g., by hand pouring, casting, or spreading on a casting surface) or automatically (e.g., by pouring or additional casting on a moving bed). Various devices known in the art can be used for casting. Casting equipment includes, for example, mechanical coaters, which include a coating knife, a doctor blade, or a spray / pressurization system. Various casting speeds are suitable as known in the art, such as casting speeds of about 2 to 6 feet per minute (fpm), depending on the specific circumstances. Preferably, the carrier temperature is 2 to 10°C lower than the temperature of the first casting solution. The first casting solution (a dilute solution with low solid content) is in direct contact with the carrier. Due to the relatively low carrier temperature, it is beneficial for the abrupt formation of the isolation layer. However, the carrier temperature should not be too low, otherwise the first casting solution may easily undergo phase separation, which may result in the formation of pores and affect the overall flux of the membrane.
[0070] Preferably, a microporous membrane support layer can be coated on the bilayer liquid film formed in S1. The film-forming material of the microporous membrane support layer is at least one of PVDF, PES, PTFE, nylon, cellulose, and polyolefin. The thickness of the microporous membrane support layer is not less than 50 μm. The porosity of the microporous membrane support layer is 30%-70%. The microporous membrane support layer contains supporting fibers for forming a porous structure, and the SEM average diameter of the supporting fibers is not less than 50 nm. The presence of the microporous membrane support layer is beneficial to greatly improving the mechanical strength of the composite membrane, making it easier to process the composite membrane and manufacture corresponding components.
[0071] To maximize the flux of the composite membrane, filter more fluid in a shorter time, and achieve higher economic efficiency per unit time, this invention pre-treats the liquid membrane by performing phase separation and solidification. Specifically, it involves pre-phase separation, where the liquid membrane is immersed in a pre-phase separation solution. This solution is a mixture of a good solvent and a non-solvent. The good solvent is miscible with both organic solvents (a first organic solvent and a second organic solvent), and the good solvent can be the same as or different from the organic solvent. The non-solvent is water or ethanol. The presence of the non-solvent helps the liquid membrane near the air side to undergo initial phase separation. Since the non-solvent content is relatively low (20%–40%), the liquid membrane undergoes slow phase separation, which facilitates the formation of larger pores in the region near the air side. Furthermore, the pre-phase separation process... The presence of larger pores near the air side allows the coagulation bath to penetrate more easily into the liquid film near the carrier side, resulting in more complete phase separation. This leads to a composite membrane with higher porosity and consequently, higher flux. In this invention, the pre-phase separation time is 2–10 seconds. The synergistic effect of the pre-phase separation time, the type of pre-phase separation liquid, and the casting solution formulation facilitates the formation of a composite membrane with relatively high porosity. It also helps to obtain an ideal membrane pore structure and pore size (such as obtaining a separation layer with a basically symmetrical structure). Preferably, the temperature of the pre-phase separation liquid is 2–15°C higher than the temperature of the second casting solution. A slightly higher pre-phase separation liquid temperature makes it easier to ensure uniform membrane pores, which is more conducive to maintaining the basic symmetrical structure of the separation layer, thus resulting in a membrane with high retention efficiency.
[0072] The pre-phase-separated bilayer liquid film is then immersed in a coagulation bath for phase separation and solidification. The solidification time is 20–60 s to obtain a green film. The coagulation bath is water, and the preferred temperature is 15–45 °C. Through the ideal phase separation and solidification process, a green film with an ideal membrane structure is finally obtained. The green film is then placed in a 0.01 mol / L–0.1 mol / L sodium hydroxide aqueous solution for hydrolysis (hydrolysis temperature 20–50 °C, hydrolysis time 40–120 min). After hydrolysis, the film is washed to form a solid film. This solid film has better hydrophilicity and lower non-specific adsorption of proteins, thereby further improving protein yield and economic benefits.
[0073] One of the characteristics of cellulose is its soft texture, which often results in cellulose membranes obtained after hydrolysis and regeneration having poor mechanical properties. Virus removal filtration often employs dead-end filtration, which subjectes the membrane to significant pressure from the feed solution. If the membrane's pressure resistance is insufficient, it may cause the membrane pore structure to collapse. Once the membrane's pore structure collapses due to pressure, its virus retention capacity and flux will be significantly affected. Therefore, the membrane is further cross-linked with a cross-linking agent (at least one of halogenated epoxides, dihaloalkanes, and dihaloalcohols) to improve the membrane's pressure resistance and reduce the possibility of structural collapse under pressure. During the cross-linking modification process, the hydroxyl groups in the membrane react with functional groups such as epoxy and halogens, thereby increasing the membrane's mechanical strength, making it less prone to swelling, and also improving its alkali resistance and service life, ultimately forming a virus removal membrane with excellent performance in all aspects.
[0074] The beneficial effects of this invention are as follows: The cellulose virus-removing composite membrane provided by this invention includes a main body, which comprises a pre-filtration layer, a separation layer, and an isolation layer for isolating and protecting the separation layer. One side of the isolation layer is a second outer surface, on which there are several second pores, the average SEM pore size of which is 50-500 nm. The isolation layer contains isolation fibers for forming a porous structure, the average SEM diameter of which is 20-120 nm. The second pores with suitable pore size and the isolation fibers with suitable fiber thickness work together to isolate and protect the separation layer during the membrane preparation and peeling process, avoiding various damages to the separation layer and thus affecting the top wash LRV. The final cellulose virus-removing composite membrane, while ensuring high retention efficiency, still has a top wash LRV greater than 4, that is, the top wash LRV consistency of the membrane batch is high, ensuring high protein yield. In addition, the isolation layer is very thin, ensuring that the composite membrane also has good flux. Furthermore, this invention also provides a method for preparing the composite membrane, which is convenient, fast, effective, simple to operate, environmentally friendly, and suitable for large-scale promotion. Attached Figure Description
[0075] Figure 1 The image shows a scanning electron microscope (SEM) image of the first outer surface of the composite film prepared in Example 1, with a magnification of 10K×.
[0076] Figure 2 The image shown is a further magnified scanning electron microscope (SEM) image of the first outer surface of the composite film prepared in Example 1, with a magnification of 20K×.
[0077] Figure 3 The image shows a scanning electron microscope (SEM) image of the second outer surface of the composite film prepared in Example 1, with a magnification of 10K×.
[0078] Figure 4The image shown is a further magnified scanning electron microscope (SEM) image of the second outer surface of the composite film prepared in Example 1, with a magnification of 20K×.
[0079] Figure 5 The image shows a scanning electron microscope (SEM) image of the longitudinal section of the composite membrane prepared in Example 1 near the liquid outlet surface, with a magnification of 10K×.
[0080] Figure 6 The image shown is a further magnified scanning electron microscope (SEM) image of the longitudinal section of the composite membrane prepared in Example 1, near the liquid outlet surface, with a magnification of 20K×. Detailed Implementation
[0081] To more clearly illustrate the overall concept of this application, detailed descriptions are provided below using examples. Unless otherwise specified, the raw materials and equipment used to prepare the composite membrane in the following examples are commercially available. Specifically, a Hitachi S-5500 scanning electron microscope was used to characterize the structural morphology of the composite membrane.
[0082] Example 1
[0083] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0084] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; wherein the temperature of the carrier is 8°C lower than the temperature of the first casting solution.
[0085] The first casting solution comprises the following raw materials in parts by weight: 18 parts of the first film-forming polymer, 100 parts of the first organic solvent, and 30 parts of the first pore-forming agent;
[0086] The second casting solution comprises the following raw materials in parts by weight: 30 parts of the second film-forming polymer, 45 parts of the second organic solvent, and 20 parts of the second pore-forming agent;
[0087] The first and second film-forming polymers are both cellulose triacetate; the first and second organic solvents are both acetone; the first pore-forming agent is polyvinylpyrrolidone; and the second pore-forming agent is ethanol; the temperature of the first and second casting solutions is 20°C; the viscosity of the first casting solution is 7000 mPa·s; and the viscosity of the second casting solution is 28000 mPa·s.
[0088] S2: The double-layer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 3s; the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 40%; the good solvent is acetone and the non-solvent is water; the temperature of the pre-phase separation liquid is 12℃ higher than the temperature of the second casting liquid.
[0089] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 25s to obtain a green film. The coagulation bath is water and the temperature of the coagulation bath is 35℃.
[0090] S4. Place the biofilm in an aqueous sodium hydroxide solution for hydrolysis, and wash after hydrolysis to form a biofilm.
[0091] Example 2
[0092] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0093] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; wherein the temperature of the carrier is 7°C lower than the temperature of the first casting solution.
[0094] The first casting solution comprises the following raw materials in parts by weight: 16 parts of the first film-forming polymer, 120 parts of the first organic solvent, and 35 parts of the first pore-forming agent; the second casting solution comprises the following raw materials in parts by weight: 27 parts of the second film-forming polymer, 50 parts of the second organic solvent, and 24 parts of the second pore-forming agent.
[0095] The first and second film-forming polymers are both cellulose diacetate; the first and second organic solvents are both dioxane; the first pore-forming agent is polyvinyl alcohol; and the second pore-forming agent is isopropanol; the temperature of the first and second casting solutions is 20°C.
[0096] The viscosity of the first casting solution is 6500 mPa·s; the viscosity of the second casting solution is 26000 mPa·s.
[0097] S2: The double-layer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 4s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 36%; the good solvent is dioxane, and the non-solvent is water; the temperature of the pre-phase separation liquid is 12°C higher than the temperature of the second casting liquid.
[0098] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 30s to obtain a green film. The coagulation bath is water and the temperature of the coagulation bath is 35℃.
[0099] S4. Place the biofilm in an aqueous sodium hydroxide solution for hydrolysis, and wash after hydrolysis to form a biofilm.
[0100] Example 3
[0101] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0102] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; wherein the temperature of the carrier is 6°C lower than the temperature of the first casting solution.
[0103] The first casting solution comprises the following raw materials in parts by weight: 15 parts of the first film-forming polymer, 130 parts of the first organic solvent, and 40 parts of the first pore-forming agent; the second casting solution comprises the following raw materials in parts by weight: 25 parts of the second film-forming polymer, 55 parts of the second organic solvent, and 28 parts of the second pore-forming agent.
[0104] The first and second film-forming polymers are both cellulose acetate butyrate; the first and second organic solvents are both dimethylacetamide; the first pore-forming agent is polyethylene glycol; and the second pore-forming agent is n-butanol; the temperature of the first and second casting solutions is 25°C; the viscosity of the first casting solution is 6000 mPa·s; and the viscosity of the second casting solution is 24000 mPa·s.
[0105] S2: The double-layer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 5s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 32%; the good solvent is dimethylacetamide, and the non-solvent is water; the temperature of the pre-phase separation liquid is 8°C higher than the temperature of the second casting liquid;
[0106] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 35s to obtain a green film. The coagulation bath is water and the temperature of the coagulation bath is 30℃.
[0107] S4. The film is placed in an aqueous sodium hydroxide solution for hydrolysis. After hydrolysis, it is washed to form a film. The film is then subjected to crosslinking treatment in a crosslinking agent. After the crosslinking treatment is completed and the film is washed, a composite film is obtained. The crosslinking agent is a halogenated epoxide.
[0108] Example 4
[0109] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0110] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; then cover the double-layer liquid film with a microporous membrane support layer, the film-forming material of the microporous membrane support layer is nylon, and the thickness is 70μm; wherein the temperature of the carrier is 4℃ lower than the temperature of the first casting solution.
[0111] The first casting solution comprises the following raw materials in parts by weight: 14 parts of the first film-forming polymer, 150 parts of the first organic solvent, and 45 parts of the first pore-forming agent;
[0112] The second casting solution comprises the following raw materials in parts by weight: 22 parts of the second film-forming polymer, 60 parts of the second organic solvent, and 32 parts of the second pore-forming agent;
[0113] The first and second film-forming polymers are both cellulose triacetate; the first and second organic solvents are both N-methylpyrrolidone; the first pore-forming agent is polypropylene glycol; and the second pore-forming agent is 1-pentanol; the temperature of the first and second casting solutions is 30°C; the viscosity of the first casting solution is 5000 mPa·s; and the viscosity of the second casting solution is 20000 mPa·s.
[0114] S2: The double-layer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 8s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, wherein the mass content of the non-solvent is 28%; the good solvent is N-methylpyrrolidone, and the non-solvent is water; the temperature of the pre-phase separation liquid is 8°C higher than the temperature of the second casting liquid.
[0115] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 45s to obtain a green film. The coagulation bath is water and the temperature of the coagulation bath is 30℃.
[0116] S4. Place the biofilm in an aqueous sodium hydroxide solution for hydrolysis, and wash after hydrolysis to form a biofilm.
[0117] Example 5
[0118] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0119] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; then cover the double-layer liquid film with a microporous membrane support layer, the film-forming material of the microporous membrane support layer is nylon, and the thickness is 90μm; wherein the carrier temperature is 3℃ lower than the temperature of the first casting solution.
[0120] The first casting solution comprises the following raw materials in parts by weight: 13 parts of the first film-forming polymer, 160 parts of the first organic solvent, and 48 parts of the first pore-forming agent; the second casting solution comprises the following raw materials in parts by weight: 21 parts of the second film-forming polymer, 65 parts of the second organic solvent, and 36 parts of the second pore-forming agent.
[0121] The first and second film-forming polymers are both cellulose propionate; the first and second organic solvents are both propionic acid; the first pore-forming agent is polyvinylpyrrolidone; and the second pore-forming agent is diethylamine; the temperature of the first and second casting solutions is 30°C.
[0122] The viscosity of the first casting solution is 4500 mPa·s; the viscosity of the second casting solution is 18000 mPa·s.
[0123] S2: The double-layer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 9s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, wherein the mass content of the non-solvent is 24%; the good solvent is propionic acid, and the non-solvent is water; the temperature of the pre-phase separation liquid is 5°C higher than the temperature of the second casting liquid.
[0124] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 50s to obtain a green film. The coagulation bath is water. The temperature of the coagulation bath is 25℃.
[0125] S4. Place the biofilm in an aqueous sodium hydroxide solution for hydrolysis, and wash after hydrolysis to form a biofilm.
[0126] Example 6
[0127] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0128] S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; then cover the double-layer liquid film with a microporous membrane support layer, the film-forming material of the microporous membrane support layer is nylon, and the thickness is 100μm; wherein the temperature of the carrier is 2℃ lower than the temperature of the first casting solution.
[0129] The first casting solution comprises the following raw materials in parts by weight: 12 parts of a first film-forming polymer, 180 parts of a first organic solvent, and 50 parts of a first pore-forming agent; the second casting solution comprises the following raw materials in parts by weight: 20 parts of a second film-forming polymer, 70 parts of a second organic solvent, and 40 parts of a second pore-forming agent; wherein both the first and second film-forming polymers are cellulose diacetate; both the first and second organic solvents are acetone; the first pore-forming agent is polyethylene glycol; and the second pore-forming agent is formamide; the temperature of both the first and second casting solutions is 35°C; the viscosity of the first casting solution is 4000 mPa·s; and the viscosity of the second casting solution is 15000 mPa·s.
[0130] S2: The double-layer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 10s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 20%; the good solvent is acetone, and the non-solvent is water; the temperature of the pre-phase separation liquid is 5°C higher than the temperature of the second casting liquid.
[0131] S3. The double-layer liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 55s to obtain a green film. The coagulation bath is water and the temperature of the coagulation bath is 20℃.
[0132] S4. The film is placed in an aqueous sodium hydroxide solution for hydrolysis. After hydrolysis, it is washed to form a film. Finally, the film is cross-linked in a cross-linking agent. After the cross-linking treatment is completed and the film is washed, a composite film is obtained. The cross-linking agent is a dihaloalkane.
[0133] Comparative Example 1
[0134] A method for preparing a cellulose virus-removing composite membrane includes the following steps:
[0135] S1. Prepare a casting solution and cast it onto a carrier to form a liquid film. The casting solution comprises the following raw materials in parts by weight: 30 parts of film-forming polymer, 45 parts of organic solvent, and 20 parts of pore-forming agent. The film-forming polymer is cellulose triacetate; the organic solvent is acetone; and the pore-forming agent is ethanol. The temperature of the casting solution is 20°C, and the viscosity of the casting solution is 28000 mPa·s.
[0136] S2: The liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 3s; the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 40%; the good solvent is acetone and the non-solvent is water; the temperature of the pre-phase separation liquid is 12℃ higher than the temperature of the casting liquid.
[0137] S3. The liquid film is immersed in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 25s to obtain a green film. The coagulation bath is water and the temperature of the coagulation bath is 35℃.
[0138] S4. Place the biofilm in an aqueous sodium hydroxide solution for hydrolysis, and wash after hydrolysis to form a biofilm.
[0139] Comparative Example 2
[0140] The virus-removing composite membrane was prepared in Example 1 using the patent publication number CN116236925A - An Asymmetric Regenerated Cellulose Virus-Removing Composite Membrane and Its Preparation Process.
[0141] 1. Structural Characterization
[0142] The morphology of the composite membranes obtained in each embodiment was characterized using scanning electron microscopy, and the required data were then obtained; the specific results are shown in the table below:
[0143] Table 1:
[0144]
[0145] Table 2:
[0146]
[0147] Table 3:
[0148]
[0149] Table 4:
[0150] SEM average pore size of the first outer surface (nm) The percentage of the void area on the first outer surface Example 1 400 16 Example 2 600 18 Example 3 900 21
[0151] As shown in the table above, the virus-removing composite membranes prepared in Examples 1-6 all have ideal membrane structures and contain an isolation layer. The isolation layer protects the separation layer during the membrane preparation and peeling process, preventing damage to the separation layer and thus affecting the top wash LRV. The final cellulose virus-removing composite membrane maintains a high retention efficiency while still having a top wash LRV greater than 4, and the top wash LRV of the membrane batches is highly consistent, ensuring a high protein yield. In addition, the isolation layer is very thin, which also gives the composite membrane good flux.
[0152] Performance characteristics
[0153] The viral challenge test was performed according to the relevant specifications in PDA TR41, using PP7 bacteriophage or hepatitis B virus as the model virus, IVIG as the model protein, and PBS as the buffer. During the test, the flux change over time was recorded, yielding the filter membrane's LRV and flux. When the filter membrane flux decreased to 25% or when only a small amount of the challenge solution remained at the bottom, a top wash was performed. Specifically, the external pressure was removed, buffer was added, and the mixture was allowed to stand for 15 minutes. Then, the pressure was increased to 30 psi for the post-process hold viral challenge test. The collected filtrate at this point was the top wash filtrate. The top wash filtrate was collected separately, and the viral titer was determined. The LRV after top washing was calculated to further determine the top wash LRV retention factor.
[0154] Flux / LMH@30psi Example 1 80 Example 2 90 Example 3 100 Example 4 110 Example 5 130 Example 6 120 Comparative Example 1 82
[0155] As shown in the table above, the composite membranes prepared in Examples 1-6 all exhibit good flux, meeting the needs of practical applications. A comparison between Example 1 and Comparative Example 1 reveals that the presence of the isolation layer in Example 1 has almost no impact on the overall membrane flux, effectively achieving both isolation and protection of the separation layer and a high membrane flux simultaneously. Furthermore, we found that in the initial LRV test, the retention efficiencies of Example 1 and Comparative Example 1 were essentially the same (LRV values were roughly identical).
[0156] Furthermore, we conducted a top-wash LRV test on the same batch of membranes (100 sheets). When the top-wash LRV was greater than 4, we considered the product to be qualified and finally calculated the pass rate.
[0157] Pass rate / % Example 1 98 Example 2 96 Example 3 99 Example 4 96 Example 5 97 Example 6 98 Comparative Example 1 70 Comparative Example 2 75
[0158] As shown in the table above, the composite membranes prepared in Examples 1-6 have almost all top-wash LRV values greater than 4 due to the presence of the isolation layer. While Comparative Examples 1 and 2 have high initial retention efficiencies, the absence of an isolation layer damages the separation layer of some membranes, affecting their top-wash LRV values. This results in some membranes having top-wash LRV values less than 4, impacting the consistency of top-wash LRV values between batches. The comparison between Example 1 and Comparative Examples 1-2 demonstrates that the presence of the isolation layer effectively protects the separation layer during the preparation and peeling process, ensuring a large top-wash LRV value for the membranes. This ensures that the top-wash LRV values of membranes from the same batch are essentially the same, exhibiting high consistency and further meeting the needs of practical applications, resulting in high economic benefits.
[0159] Furthermore, according to the test method used in paragraph 114 of CN201010154974.7-Supercomposite membrane and its preparation method: virus retention test was performed: the virus used was mouse parvovirus with a particle size of 20nm;
[0160] After testing, it was found that the composite membranes prepared in Examples 1-6 had an LRV of no less than 4 for viral impurities with a particle size of 20 nm, thus demonstrating that the composite membrane of the present invention has sufficient retention capacity for viruses of 20 nm and above; and the protein yield of the composite membrane is no less than 98%; therefore, this composite membrane is particularly suitable for application in the field of virus removal. Furthermore, the interception efficiency of the composite membranes obtained in each example was tested; intercepted particles: colloidal gold with a particle size of 20 nm; after testing, it was found that the samples prepared in Examples 1-6 had a retention efficiency of no less than 99.99% for colloidal gold with a particle size of 20 nm.
[0161] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A cellulose virus-removing composite membrane, comprising a body having non-directional tortuous pathways within the body, one side surface of the body being a first outer surface, and the other side surface of the body being a second outer surface, characterized in that: The main body includes a pre-filter layer, a separation layer for intercepting viruses, and an isolation layer for isolating and protecting the separation layer. The pre-filter layer is located on the side of the separation layer away from the isolation layer, and one side of the isolation layer is a second outer surface. The average pore size of the isolation layer is larger than the average pore size of the separation layer. The second outer surface has a plurality of second holes, and the average SEM pore size of the second holes is 50~500nm; The isolation layer contains isolation fibers for forming a porous structure, and the average SEM diameter of the isolation fibers is 20~120nm; the thickness of the isolation layer is not higher than 10μm. The average PMI pore size of the composite membrane is 15~30nm; For PP7 bacteriophage, the top wash LRV of the composite membrane is not less than 4; The aperture variation coefficient S of the isolation layer (0.9~1) / (0~0.1) No less than 3; The aperture variation coefficient of the isolation layer refers to that the isolation layer region is divided into 10 parts according to the thickness, the side close to the first outer surface is regarded as the region 0, and the second outer surface is regarded as the region 1. The aperture of a plurality of holes in each region is measured according to actual needs, and then the average value is taken. The value is the average aperture of the region. The aperture variation coefficient S x / y ; The ratio of the thickness of the isolation layer to the thickness of the separation layer is 1:10~40.
2. The virus-free composite membrane of fibers according to claim 1, characterized in that: The thickness of the isolation layer is 0.2~5μm; the thickness of the isolation layer does not exceed 15% of the overall thickness of the membrane; and the porosity of the isolation layer is not less than 20%.
3. The virus-free composite membrane of claim 1, wherein: The area ratio of the pores on the second outer surface is 3% to 40%; some adjacent second pores are separated by surface fibers, and the average SEM width of the surface fibers is 15 to 100 nm.
4. The virus-free composite membrane of claim 1, wherein: The aperture variation coefficient S of the isolation layer (0.9~1) / (0~0.1) Not less than 5.
5. The virus-free composite membrane of claim 4, wherein: The aperture variation coefficient S of the isolation layer is 1.1-2; and / or, the aperture variation coefficient S of the isolation layer is 3-20. (0.4~0.5) / (0~0.1) The aperture variation coefficient S of the isolation layer is 1.1-2; and / or, the aperture variation coefficient S of the isolation layer is 3-20. (0.9~1) / (0.5~0.6) The aperture variation coefficient S of the isolation layer is 1.1-2; and / or, the aperture variation coefficient S of 6. The cellulose virus-removing composite membrane according to claim 4, characterized in that: The pore size variation coefficient S of the isolation layer (0.4~0.5) / (0~0.1) The pore size variation coefficient S of the isolation layer (0.9~1) / (0.5~0.6) The ratio of the two is 1:1.5 to 8.
7. The virus-free composite membrane of claim 1, wherein: The separation layer has a basically symmetrical structure; the separation layer contains retained fibers for forming a porous structure, and the SEM average diameter of the retained fibers is 15~100nm; The ratio of the average SEM diameter of the isolation fiber to the average SEM diameter of the retained fiber is 1.05 to 3:
1.
8. The cellulose virus-removing composite membrane according to claim 1, characterized in that: The average SEM pore size of the separation layer is 25~80nm, and the ratio of the average SEM pore size of the isolation layer to the average SEM pore size of the separation layer is not less than 3.
9. The cellulose virus-removing composite membrane according to claim 1, characterized in that: The thickness of the separation layer is 15~60μm.
10. The cellulose virus-removing composite membrane according to claim 1, characterized in that: The average pore size of the pre-filter layer is greater than the average pore size of the isolation layer; The pre-filter layer contains pre-filter fibers for forming a porous structure, and the SEM average diameter of the pre-filter fibers is 30~150nm. The ratio of the SEM average diameter of the pre-filtered fiber to the SEM average diameter of the isolation fiber is 1.1 to 4.
11. The cellulose virus-removing composite membrane according to claim 1, characterized in that: One side of the pre-filter layer is a first outer surface, the average SEM pore size of the first outer surface is 200~4000nm, and the pore area ratio of the first outer surface is 5%~45%.
12. The cellulose virus-removing composite membrane according to claim 1, characterized in that: The main body also includes a microporous membrane support layer, one side of which is a first outer surface. The thickness of the microporous membrane support layer is not less than 50 μm, and the porosity of the microporous membrane support layer is 30% to 70%. The microporous membrane support layer contains supporting fibers for forming a porous structure, and the SEM average diameter of the supporting fibers is not less than 50 nm.
13. The cellulose virus-removing composite membrane according to claim 1, characterized in that: The composite membrane has a thickness of 50~300μm and a porosity of 20%~55%. The flux of the composite membrane is 45~150 L*h. -1 *m -2 @30psi; The composite membrane has an LRV of not less than 4 for PP7 phage; The protein yield of the composite membrane is not less than 98%.
14. A method for preparing a cellulose virus-removing composite membrane according to any one of claims 1-13, characterized in that: Includes the following steps: S1. Prepare a first casting solution and a second casting solution, and sequentially cast the first casting solution and the second casting solution onto a carrier to form a double-layer liquid film; the temperature of the carrier is 2~10℃ lower than the temperature of the first casting solution. The first casting solution comprises the following raw materials in parts by weight: 10-20 parts of the first film-forming polymer, 50-200 parts of the first organic solvent, and 20-60 parts of the first pore-forming agent; The second casting solution comprises the following raw materials in parts by weight: 10-30 parts of the second film-forming polymer, 30-80 parts of the second organic solvent, and 20-40 parts of the second pore-forming agent; Both the first film-forming polymer and the second film-forming polymer are cellulose polymers; the viscosity ratio of the first casting solution to the viscosity of the second casting solution is 1:(2~6). S2: The bilayer liquid film is immersed in the pre-phase separation liquid for pre-phase separation, and the pre-phase separation time is 2~10s; wherein the pre-phase separation liquid includes a good solvent and a non-solvent, and the mass content of the non-solvent is 20%~40%; the good solvent is at least one of acetone, dioxane, dimethylacetamide, N-methylpyrrolidone, acetic acid, propionic acid, butyric acid and valeric acid, and the non-solvent is water or ethanol; S3. Immerse the double-layer liquid film in a coagulation bath for phase separation and solidification. The phase separation and solidification time is 20~60s to obtain a green film. The coagulation bath is water. S4. Place the biofilm in an aqueous sodium hydroxide solution for hydrolysis, and wash after hydrolysis to form a biofilm.
15. The method for preparing a cellulose virus-removing composite membrane according to claim 14, characterized in that: The temperatures of the first and second casting solutions are 15~40℃; the viscosity of the first casting solution is 3000~8000 mPa·s; and the viscosity of the second casting solution is 10000~30000 mPa·s. The first organic solvent and the second organic solvent are at least one of acetone, dioxane, dimethylacetamide, N-methylpyrrolidone, acetic acid, propionic acid, butyric acid and valeric acid; The first pore-forming agent is at least one of polyvinylpyrrolidone, polyvinyl alcohol, polyethylene glycol, and polypropylene glycol; The second pore-forming agent is any one of formamide, ethanol, 1-propanol, isopropanol, n-butanol, 1-pentanol, 2-pentanol, and diethylamine.
16. The method for preparing a cellulose virus-removing composite membrane according to claim 14, characterized in that: A microporous membrane support layer is coated on the bilayer liquid film formed in S1. The film-forming material of the microporous membrane support layer is at least one of PVDF, PES, PTFE, nylon, cellulose and polyolefin; the polyolefin is UPE or PP.
17. The method for preparing a cellulose virus-removing composite membrane according to claim 14, characterized in that: The temperature of the pre-phase separation liquid is 2-15°C higher than that of the second casting liquid; the temperature of the coagulation bath is 15-45°C.
18. The method for preparing a cellulose virus-removing composite membrane according to claim 14, characterized in that: The film obtained by S4 is cross-linked in a cross-linking agent. After the cross-linking treatment is completed and the film is cleaned, a composite film is obtained. The cross-linking agent is at least one of haloepoxide, dihaloalkanes and dihaloalcohols.
Citation Information
Patent Citations
Ultrafiltration membrane and manufacturing method
CN101816898B
Remove the viral membrane
CN105980037B
Asymmetric copper ammonia cellulose filter membrane for removing viruses and preparation process of asymmetric copper ammonia cellulose filter membrane
CN116116247A
Ultrafiltration membrane and preparation method thereof
CN1759924A
Cellulose virus-removing membrane with high virus rejection rate and preparation process of cellulose virus-removing membrane