A metal crosslinked polybenzimidazole hydrogen separation membrane and its preparation method
By introducing trivalent chromium, aluminum, or iron ions into the nitrogen heterocycle of polybenzimidazole to form a cross-linked network structure, the problem of insufficient H2/CO2 separation performance of existing polybenzimidazole membranes is solved, and a highly efficient hydrogen separation effect is achieved.
Patent Information
- Application Number
- CN202311647432.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-01
AI Technical Summary
Existing polybenzimidazole hydrogen separation membranes are insufficient in H2/CO2 separation performance, which limits their application in hydrogen separation.
By coordinating polybenzimidazole nitrogen heterocycles with trivalent chromium, aluminum, or iron ions to form a cross-linked network structure, the temperature, concentration, and pH of the aqueous solution of metal ions can be adjusted to form a polynuclear complex, thereby enhancing gas sieving performance.
It significantly improves the selectivity and performance of hydrogen separation membranes, hinders the diffusion of large molecular gases, and achieves highly efficient hydrogen separation.
Smart Images

Figure CN117753234B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a metal crosslinked polybenzimidazole hydrogen separation membrane and its preparation method, belonging to the field of gas separation technology. Background Technology
[0002] Driven by global population growth and economic development, the global energy landscape is changing. Clean energy is receiving increasing attention. Hydrogen (H2) is a green fuel with high energy density, and its combustion byproduct is only water, causing no damage to the environment or ecosystem. The utilization of hydrogen will play a crucial role in decarbonization and sustainable development. However, currently, most hydrogen is produced through fossil fuel reforming or gasification, with carbon dioxide (CO2) as the main byproduct, along with small amounts of methane (CH4) and other byproducts. Therefore, the separation of high-temperature syngas is essential.
[0003] Hydrogen separation and purification can be achieved through various methods, including pressure swing adsorption (PSA), cryogenic distillation, and gas membrane separation. PSA involves high-pressure adsorption, utilizing the adsorption-desorption mechanism (pressure adsorption-depressurization desorption) to selectively adsorb gases in a limited space using suitable adsorbents, such as zeolite or activated carbon. Cryogenic distillation is another widely mentioned gas separation method. During cryogenic distillation, the mixed gases are condensed and separated according to their boiling points. In contrast, gas membrane separation is a high-tech method that has shown great potential in the hydrogen separation market. It has the following characteristics: (1) high energy efficiency; (2) low cost; (3) simple operation; (4) convenience; (5) environmental friendliness. Furthermore, membrane separation technology can be combined with other gas separation processes to obtain better hydrogen separation processes. Gas separation membrane materials include: inorganic membrane materials, organic (polymer membrane materials), and organic-inorganic hybrid membrane materials. Among them, polymer membrane materials have excellent processing performance and are widely used in gas membrane separation. Although the dynamic diameter of H2... Compared to CO2 O2 N2 and CH4 However, the small size of the carbon dioxide (PCD) makes H2 difficult to condense, resulting in low selectivity for hydrogen in traditional polymers, which limits their application in hydrogen separation. Polybenzimidazole (PB) is a glassy polymer. Due to the rigid structure of the imidazole ring and the strong hydrogen bonding between chain segments, it has strong sieving ability and high thermal stability, making it suitable for the high-temperature environment of syngas. It is an ideal hydrogen separation membrane material. However, the H2 / CO2 separation performance of existing PB membranes is still insufficient, which remains a challenge in the process of industrial application. Summary of the Invention
[0004] To address the shortcomings and deficiencies of existing technologies, the present invention aims to provide a metal-crosslinked polybenzimidazole hydrogen separation membrane and its preparation method. This hydrogen separation membrane enhances gas sieving performance by coordinating the nitrogen heterocycles of polybenzimidazole with trivalent chromium, aluminum, or iron ions in an aqueous solution to form a crosslinked network structure. By adjusting conditions such as the temperature, metal ion concentration, and pH of the metal ion aqueous solution, trivalent chromium, aluminum, or iron ions undergo hydration, hydrolysis, and polymerization processes in the solution to form polynuclear complexes. These complexes then coordinate and crosslink with nitrogen atoms on multiple polybenzimidazole molecular chains, forming a multi-point crosslinked network. This significantly improves the gas size sieving performance of the membrane, thereby enhancing the hydrogen separation performance of the polybenzimidazole hydrogen separation membrane.
[0005] The first objective of this invention is to provide a metal-crosslinked polybenzimidazole hydrogen separation membrane, wherein the metal-crosslinked polybenzimidazole hydrogen separation membrane has a crosslinked network structure formed by the coordination of polybenzimidazole and metal ions, wherein the metal ions are one or more selected from chromium, aluminum, and iron; the thickness of the metal-crosslinked polybenzimidazole hydrogen separation membrane is 10–30 μm; the mass concentration of metal ions in the metal-crosslinked polybenzimidazole hydrogen separation membrane is 0.5–4 wt%; and the crosslinking percentage of metal ions in the metal-crosslinked polybenzimidazole hydrogen separation membrane is 5–35%.
[0006] In one embodiment, the metal ion has a valence state of +3 and a coordination number of 6.
[0007] In one embodiment, the polybenzimidazole is an aryl ether polybenzimidazole or a fully aromatic polybenzimidazole.
[0008] In one embodiment, the structural formula of the aromatic ether type polybenzimidazole is: Molecular weight ranges from 10,000 to 100,000.
[0009] In one embodiment, the structural formula of the fully aromatic polybenzimidazole is: Molecular weight ranges from 10,000 to 100,000.
[0010] A second objective of this invention is to provide a method for preparing the metal crosslinked polybenzimidazole hydrogen separation membrane described above, the method comprising the following steps:
[0011] (1) Dissolve polybenzimidazole in a polar organic solvent and dissolve at 50-80℃ for 10-24h to prepare a casting solution with a mass concentration of 6-12wt%; after coating the casting solution onto a glass plate, dry it at 30-80℃ for 12-24h to obtain a polybenzimidazole film.
[0012] (2) Prepare a metal salt solution with a concentration of 0.01 to 0.30 mmol / g using a methanol / water mixture and adjust the pH value to 2 to 7; immerse the polybenzimidazole membrane prepared in step (1) in the metal salt solution for in-situ coordination crosslinking, take it out and rinse it with methanol, and dry it in an oven at 30 to 50°C for 12 to 24 hours to obtain the metal crosslinked polybenzimidazole hydrogen separation membrane.
[0013] In one embodiment, the polar organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, or N-methylpyrrolidone.
[0014] In one embodiment, the pH value is 2 to 5.
[0015] In one embodiment, the volume ratio of methanol to water in the methanol / water mixture is 1:5 to 5:1.
[0016] In one embodiment, the metal salt is one or more of aluminum chloride, chromium chloride, ferric chloride, aluminum sulfate, chromium sulfate, ferric sulfate, aluminum nitrate, chromium nitrate, and ferric nitrate.
[0017] In one embodiment, the in-situ coordination crosslinking time is 1–48 h and the temperature is 20–40 °C.
[0018] A third objective of this invention is to provide a hydrogen separation method, wherein the method employs the aforementioned metal crosslinked polybenzimidazole hydrogen separation membrane for hydrogen separation.
[0019] In one embodiment, the hydrogen separation is performed at a temperature of 30–35°C and a pressure of 0.4–0.6 MPa.
[0020] Advantages and effects of the present invention:
[0021] 1. The polybenzimidazole hydrogen separation membrane provided by the present invention enhances gas sieving performance by forming a cross-linked network structure through the coordination of the nitrogen heterocycle of polybenzimidazole with metal ions, hinders the diffusion of macromolecular gases (such as carbon dioxide, nitrogen, methane, and oxygen), improves the hydrogen separation selectivity, and thus improves the hydrogen separation performance of the polybenzimidazole hydrogen separation membrane.
[0022] 2. The polybenzimidazole hydrogen separation membrane provided by the present invention has strong controllability of coordination crosslinking structure and uniform distribution of metal ions inside the polymer; and the metal ions used are common metal salts, which are inexpensive.
[0023] 3. The preparation method of the polybenzimidazole hydrogen separation membrane provided by the present invention uses a simple, convenient, efficient, and reproducible solid-state immersion in-situ coordination crosslinking process. Attached Figure Description
[0024] Figure 1 The image shows the infrared spectrum of a chromium cross-linked polybenzimidazole hydrogen separation membrane.
[0025] Figure 2 Scanning electron microscope (SEM) image and energy dispersive spectroscopy (EDS) image of a chromium-crosslinked polybenzimidazole hydrogen separation membrane; (a) SEM image; (b) EDS image. Detailed Implementation Plan
[0026] The technical solution of the invention will be described in detail below with reference to the accompanying drawings:
[0027] Example 1
[0028] A method for preparing a chromium crosslinked polybenzimidazole hydrogen separation membrane, the method comprising the following steps:
[0029] (1) Dissolve aryl ether type polybenzimidazole (molecular weight about 40,000) in N,N-dimethylformamide and dissolve at 80°C for 24 h to obtain a casting solution with a mass concentration of 9 wt%; coat the casting solution onto a glass plate to form a film and dry at 80°C for 12 h to obtain a polybenzimidazole film.
[0030] (2) Dissolve chromium chloride in a methanol / water mixed solvent with a volume ratio of 1:1 to prepare a chromium chloride solution with a chromium ion concentration of 0.30 mmol / g; immerse the polybenzimidazole membrane prepared in step (1) in the chromium chloride solution for in-situ coordination crosslinking for 48 h, at a temperature of 25 °C and a pH of 2.0; then, take out the membrane, rinse it with methanol, and dry it in an oven at 40 °C for 12 h to obtain the chromium crosslinked polybenzimidazole hydrogen separation membrane.
[0031] The chromium-crosslinked polybenzimidazole hydrogen separation membrane prepared in this embodiment has a thickness of 18 μm; the chromium ion mass concentration in the membrane is 4 wt%; and the chromium ion coordination crosslinking percentage of the membrane is 35%. The prepared chromium-crosslinked polybenzimidazole hydrogen separation membrane was placed in a gas permeability performance evaluation device for hydrogen separation performance testing. The test temperature was 35℃, and the test pressure was 0.4 MPa. The membrane's H2 permeability coefficient was 2.12 Barrer, the CO2 permeability coefficient was 0.13 Barrer, and the H2 / CO2 separation selectivity was 16.31.
[0032] Figure 1 The images show the infrared spectra of the chromium-crosslinked polybenzimidazole membrane and the polybenzimidazole membrane prepared in Example 1 and Comparative Example 1 of this invention. Compared with the polybenzimidazole membrane, the C=N stretching vibration peak of the imidazole ring in the chromium-crosslinked polybenzimidazole membrane is enhanced and shifted to higher wavenumbers, and the CN stretching vibration on the imidazole ring undergoes a blue shift, confirming the coordination reaction between chromium ions and the imidazole ring.
[0033] Figure 2The images show cross-sectional scanning electron microscope (SEM) images and energy dispersive spectroscopy (EDS) images of the chromium cross-linked polybenzimidazole membrane prepared in Example 1 of this invention. The cross-section of the membrane has no obvious defects, and uniformly distributed chromium elements can be seen in the cross-linked polybenzimidazole membrane.
[0034] Example 2
[0035] A method for preparing an iron-crosslinked polybenzimidazole hydrogen separation membrane, the method comprising the following steps:
[0036] (1) Dissolve fully aromatic polybenzimidazole (molecular weight of about 30,000) in N,N-dimethylformamide and dissolve at 80°C for 24 h to obtain a casting solution with a mass concentration of 12 wt%; coat the casting solution onto a glass plate to form a film and dry at 50°C for 12 h to obtain a polybenzimidazole film.
[0037] (2) Dissolve ferric chloride in a 1:2 ratio of methanol / water to prepare a ferric chloride solution with an iron ion concentration of 0.08 mmol / g; immerse the polybenzimidazole membrane prepared in step (1) in the iron ion solution for in-situ coordination crosslinking for 24 h, at a temperature of 35 °C and a pH of 4.0; then, remove the membrane, rinse it with methanol, and dry it in a 50 °C oven for 12 h to obtain the iron-crosslinked polybenzimidazole hydrogen separation membrane.
[0038] The iron-crosslinked polybenzimidazole hydrogen separation membrane prepared in this embodiment has a thickness of 28 μm; the iron ion mass concentration in the membrane is 2 wt%; and the metal ion coordination crosslinking percentage of the membrane is 20%. The prepared iron-crosslinked polybenzimidazole hydrogen separation membrane was placed in a gas permeability evaluation device for hydrogen separation performance testing at a test temperature of 35℃ and a test pressure of 0.4 MPa. The membrane's H2 permeability coefficient was 2.09 Barrer, CO2 permeability coefficient was 0.14 Barrer, and H2 / CO2 separation selectivity was 14.93.
[0039] Example 3
[0040] A method for preparing a copper crosslinked polybenzimidazole hydrogen separation membrane, the method comprising the following steps:
[0041] (1) Dissolve aryl ether type polybenzimidazole (molecular weight about 40,000) in N,N-dimethylacetamide and dissolve at 60°C for 10 h to obtain a casting solution with a mass concentration of 6 wt%; coat the casting solution onto a glass plate to form a film and dry at 60°C for 24 h to obtain a polybenzimidazole film.
[0042] (2) Dissolve aluminum chloride in a methanol / water mixture with a volume ratio of 1:5 to prepare an aluminum chloride solution with a copper ion concentration of 0.10 mmol / g; immerse the polybenzimidazole membrane prepared in step (1) in the aluminum ion solution for in-situ coordination crosslinking for 12 h, at a temperature of 30 °C and a pH of 5.0; then, take out the membrane, rinse it with methanol, and dry it in a 30 °C oven for 24 h to obtain the aluminum crosslinked polybenzimidazole hydrogen separation membrane.
[0043] The aluminum crosslinked polybenzimidazole hydrogen separation membrane prepared in this embodiment has a thickness of 15 μm; the metal ion mass concentration in the membrane is 3 wt%; and the aluminum ion coordination crosslinking percentage of the membrane is 27%. The prepared aluminum crosslinked polybenzimidazole hydrogen separation membrane was placed in a gas permeability evaluation device for hydrogen separation performance testing. The test temperature was 35℃, and the test pressure was 0.4 MPa. The membrane's H2 permeability coefficient was 2.88 Barrer, the CO2 permeability coefficient was 0.18 Barrer, and the H2 / CO2 separation selectivity was 16.00.
[0044] Comparative Example 1
[0045] Aromatic ether polybenzimidazole was dissolved in N,N-dimethylformamide and dissolved at 70°C for 24 h to obtain a casting solution with a mass concentration of 6 wt%. The casting solution was coated onto a glass plate to form a film, which was then dried at 30°C for 12 h to obtain a polybenzimidazole film.
[0046] The polybenzimidazole membrane prepared in this comparative example was placed in a gas permeability evaluation device for hydrogen separation performance testing. The test temperature was 35℃ and the test pressure was 0.4MPa. The membrane's H2 permeability coefficient was 5.73 Barrer, the CO2 permeability coefficient was 1.18 Barrer, and the H2 / CO2 separation selectivity was 4.86.
[0047] Comparative Example 2
[0048] The only difference from Example 1 is that chromium chloride in step (1) is replaced with cobalt chloride and zinc chloride. All other parameters and conditions are the same as in Example 1, and cobalt cross-linked polybenzimidazole membrane and zinc cross-linked polybenzimidazole membrane are prepared respectively.
[0049] The benzopyrazole membrane prepared in this comparative example was tested according to the method in Example 1, and the results are shown in Table 1:
[0050] Table 1 Performance results of polybenzimidazole membranes with different metal crosslinking
[0051]
[0052] Results analysis:
[0053] Compared with Comparative Example 1, the metal cross-linked polybenzimidazole membranes prepared in Example 1 all showed higher H2 / CO2 separation selectivity, indicating that the metal cross-linked polybenzimidazole membranes have excellent performance and can be applied to hydrogen separation processes.
[0054] The H2 / CO2 separation selectivity of the chromium crosslinked polybenzimidazole membrane prepared in Example 1 was higher than that of the cobalt crosslinked polybenzimidazole membrane and the zinc crosslinked polybenzimidazole membrane prepared in Comparative Example 2. This indicates that the valence state and coordination number of metal ions have a significant impact on the molecular chain structure of the crosslinked polybenzimidazole membrane. Using chromium crosslinking can significantly improve the gas sieving performance of the catalytic membrane, thereby obtaining high hydrogen selectivity. After replacing the trivalent chromium ions with a coordination number of 6 with divalent cobalt ions or zinc ions with a coordination number of 4, the hydrogen separation performance of the crosslinked polybenzimidazole membrane decreased.
[0055] The embodiments provided above are not intended to limit the scope of the invention, nor are the described steps intended to limit the order of execution. Any obvious modifications made to the invention by those skilled in the art based on existing common knowledge also fall within the scope of protection defined by the claims.
Claims
1. A hydrogen separation method characterized by, The method employs a metal-crosslinked polybenzimidazole hydrogen separation membrane for hydrogen separation; the thickness of the metal-crosslinked polybenzimidazole hydrogen separation membrane is 10~30 μm; the mass concentration of metal ions in the metal-crosslinked polybenzimidazole hydrogen separation membrane is 0.5~4 wt%; and the metal ion coordination crosslinking percentage of the metal-crosslinked polybenzimidazole hydrogen separation membrane is 20~35%. The preparation of the metal crosslinked polybenzimidazole hydrogen separation membrane includes the following steps: (1) Dissolve polybenzimidazole in a polar organic solvent and dissolve at 50~80℃ for 10~24h to prepare a casting solution with a mass concentration of 6~12wt%; after coating the casting solution onto a glass plate, dry it at 30~80℃ for 12~24h to obtain a polybenzimidazole film. The polybenzimidazole is a fully aromatic polybenzimidazole or an aromatic ether polybenzimidazole; (2) Prepare a metal salt solution with a concentration of 0.01~0.30 mmol / g using a methanol / water mixture, and adjust the pH value to 2~5; immerse the polybenzimidazole membrane in the metal salt solution for in-situ coordination crosslinking, take it out and rinse it with methanol, and dry it in an oven at 30~50℃ for 12~24h to obtain the metal crosslinked polybenzimidazole hydrogen separation membrane. The in-situ coordination crosslinking time is 12~48h, and the temperature is 20~40℃; The metal salt is one or more of aluminum chloride, chromium chloride, ferric chloride, aluminum sulfate, chromium sulfate, ferric sulfate, aluminum nitrate, chromium nitrate, and ferric nitrate.
2. The method of claim 1, wherein, The polar organic solvent is dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, or N-methylpyrrolidone.
3. The method of claim 1, wherein, The volume ratio of methanol to water in the methanol / water mixture is 1:5 to 5:1.