A corrosion-resistant oil casing and preparation method thereof
Through reasonable proportioning of chemical components and process treatments, corrosion-resistant oil casings with lower Cr content are prepared, which solves the problems of high Cr content and high cost in the existing technology, and achieves high corrosion resistance in H2S and CO2 environments. performance and low cost oil casing.
Patent Information
- Application Number
- CN202410120538.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-29
AI Technical Summary
The existing corrosion-resistant oil casing has a high Cr content, which increases the cost, and is prone to non-uniform corrosion in H2S and CO2 environments. It is difficult to meet the needs of deep wells, ultra-deep wells, and highly acidic oil and gas fields to resist H2S stress corrosion.
Using a specific combination of chemical components, including a reasonable ratio of C, Si, Mn, Cr, Mo, Ni, Cu, V, Ti, Re, Al, Ca, P, S, O, H and N, through smelting and continuous casting , hot piercing, hot rolling, quenching and tempering heat treatment, thermal straightening and hot sizing to prepare corrosion-resistant oil casing with lower Cr content and improve its corrosion resistance in H2S and CO2 environments.
A corrosion-resistant oil casing with lower Cr content and lower cost has been realized. It has high yield strength, tensile strength and good toughness. It can maintain stable performance in H2S and CO2 environments and meet the development needs of deep well oil and gas fields.
Smart Images

Figure BDA0004686594190000121 
Figure BDA0004686594190000161 
Figure BDA0004686594190000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of petroleum pipe manufacturing, and in particular to a corrosion-resistant oil casing and a preparation method thereof. Background Art
[0002] Oil and gas containing H2S and CO2 account for a large proportion of oil and gas resources. In an environment containing H2S and CO2, under the synergistic effect of corrosive media and working stress, steel materials are prone to CO2 corrosion and sulfide stress corrosion damage, which often leads to serious consequences.
[0003] In a CO2 corrosive environment, oil casing often suffers from non-uniform corrosion, resulting in a decrease in bearing capacity and even corrosion perforation and leakage. For a corrosive environment containing CO2 oil and gas, the most effective measure is to increase the content of Cr in steel. When the Cr content exceeds 12.5%, the corrosion resistance is significantly improved, but the manufacturing cost also increases exponentially. In recent years, economical oil casing with a Cr content of 3% to 5% has been used and has achieved certain application results, but its preparation cost is still high. On the other hand, the higher the material strength, the greater the probability of sulfide stress corrosion damage. With the development of deep wells, ultra-deep wells, and highly acidic oil and gas fields, not only are there high requirements for the strength and toughness of oil casing, but also for the resistance to H2S corrosion, especially the resistance to H2S stress corrosion. The strength, toughness and resistance to H2S stress corrosion of materials often show a phenomenon of trade-off, which makes the manufacture of high-strength H2S stress corrosion resistant oil casing very difficult.
[0004] Therefore, it is urgent to develop an oil casing with low Cr content, low cost and high strength that is resistant to H2S and CO2 corrosion. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a corrosion-resistant oil casing and a preparation method thereof, aiming to solve the problem of high Cr content and high composition in the existing corrosion-resistant oil casing.
[0006] The technical solution of the present invention is as follows:
[0007] In a first aspect of the present invention, a corrosion-resistant oil casing is provided, wherein the corrosion-resistant oil casing comprises the following chemical components in terms of mass percentage:
[0008] C 0.2%~0.3%, Si 0.15%~0.4%, Mn 0.3%~0.7%, Cr 1.9%~2.1%, Mo0.25%~0.45%, Ni 0%~0.25%, Cu 0%~0.25%, V 0%~0.08%, Ti 0.01%~0.03%, Re 0.001%~0.0025%, Al 0.012%~0.02%, Ca 0.012%~0.02%, P 0%~0.015%, S0%~0.005%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0009] Optionally, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0010] C 0.2%~0.25%, Si 0.15%~0.32%, Mn 0.3%~0.68%, Cr 1.9%~2.06%, Mo0.25%~0.35%, Ti 0.01%~0.02%, Re 0.001%~0.002%, Al 0.013%~0.016%, Ca0.012%~0.017%, P 0%~0.012%, S 0%~0.004%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0011] Optionally, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0012] C 0.2%~0.22%, Si 0.15%~0.24%, Mn 0.3%~0.47%, Cr 1.9%~1.99%, Mo0.25%~0.3%, Ti 0.01%~0.02%, Re 0.001%~0.002%, Al 0.013%~0.016%, Ca0.012%~0.017%, P 0%~0.012%, S 0%~0.004%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0013] Optionally, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0014] C 0.23%~0.25%, Si 0.29%~0.32%, Mn 0.51%~0.68%, Cr 2.03%~2.06%, Mo 0.32%~0.35%, Ti 0.016%~0.019%, Re 0.0013%~0.0019%, Al 0.013%~0.015%, Ca 0.013%~0.015%, P 0%~0.012%, S 0%~0.003%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0015] Optionally, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0016] C 0.25%~0.3%, Si 0.31%~0.4%, Mn 0.46%~0.7%, Cr 1.95%~2.1%, Mo0.36%~0.45%, Ni 0.15%~0.25%, Cu 0.15%~0.25%, V 0.03%~0.08%, Ti0.021%~0.03%, Re 0.0016%~0.0025%, Al 0.012%~0.02%, Ca 0.015%~0.02%, P0%~0.012%, S 0%~0.002%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0017] Optionally, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0018] C 0.25%~0.27%, Si 0.31%~0.36%, Mn 0.46%~0.49%, Cr 1.95%~1.99%, Mo 0.36%~0.39%, Ni 0.15%~0.19%, Cu 0.15%~0.21%, V 0.03%~0.05%, Ti0.021%~0.023%, Re 0.0016%~0.0025%, Al 0.012%~0.017%, Ca0.015%~0.019%, P 0%~0.012%, S 0%~0.002%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0019] Optionally, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0020] C 0.28%~0.3%, Si 0.35%~0.4%, Mn 0.55%~0.7%, Cr 2.01%~2.1%, Mo0.4%~0.45%, Ni 0.21%~0.25%, Cu 0.22%~0.25%, V 0.06%~0.08%, Ti 0.023%~0.03%, Re 0.002%~0.0023%, Al 0.017%~0.02%, Ca 0.016%~0.02%, P 0%~0.011%, S 0%~0.001%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0021] A second aspect of the present invention provides a method for preparing a corrosion-resistant oil casing, which comprises the following steps:
[0022] According to the chemical composition of the corrosion-resistant oil casing as described above, the ingredients are prepared, smelted and continuously cast to obtain a continuous casting billet;
[0023] The continuous casting billet is subjected to hot piercing and hot continuous rolling to obtain a tube billet;
[0024] The corrosion-resistant oil casing is obtained by subjecting the tube blank to tempering heat treatment, heat straightening and heat sizing.
[0025] Optionally, the step of obtaining a tube billet after hot piercing and hot rolling the continuously cast billet specifically includes:
[0026] The continuous casting billet is heated at a temperature of 1150-1250° C. for 90-120 minutes, then hot-pierced at a temperature of 1145-1200° C., hot-rolled at a temperature of 880-1150° C., and cooled to obtain a tube billet.
[0027] Optionally, after subjecting the tube blank to tempering heat treatment, heat straightening and heat sizing, the step of obtaining the corrosion-resistant oil casing specifically includes:
[0028] The final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed. After cooling, the steel is tempered at a temperature of 640-700°C for 90-120 minutes and then water-cooled; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water-cooled to obtain the corrosion-resistant oil casing; or,
[0029] The final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed. After cooling, it is tempered at a temperature of 640-700°C for 90-120 minutes and then water-cooled; it is reheated to 880-930°C, kept warm for 60-90 minutes, internal and external water spray quenching is performed, and after cooling, it is tempered at a temperature of 610-650°C for 90-120 minutes and then water-cooled; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water-cooled to obtain the corrosion-resistant oil casing.
[0030] Beneficial effects: The corrosion-resistant oil casing provided by the present invention has a low Cr content of about 2%, low cost, good CO2 and H2S corrosion resistance, good toughness, high yield strength, and the yield strength level can reach 80ksi, 95ksi, 110ksi, and 125ksi steel grade requirements. Specifically, the room temperature yield strength of the corrosion-resistant oil casing provided by the present invention is greater than 552-862MPa, the tensile strength is greater than 655-931MPa, the total elongation is greater than or equal to 14%, and the 0°C Charpy V-notch impact toughness is greater than or equal to 90J; the NACE TM 0177A method 720-hour hydrogen sulfide stress corrosion test does not produce cracks or fractures; in P CO2 ≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a, which can meet the demand for economical corrosion-resistant oil casing in the development of H2S and low CO2 oil and gas fields. DETAILED DESCRIPTION
[0031] The present invention provides a corrosion-resistant oil casing and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0033] In recent years, economical oil casing with a Cr content of 3% to 5% has been used and has achieved certain application results, but its preparation cost is still relatively high, and it is possible to further reduce the cost by optimizing the design of alloy components. Furthermore, the higher the material strength, the greater the probability of sulfide stress corrosion damage. With the development of deep wells, ultra-deep wells, and highly acidic oil and gas fields, not only are there high requirements for the strength and toughness of oil casing, but also for the resistance to H2S corrosion, especially the resistance to H2S stress corrosion. However, the strength and toughness of the material and the resistance to H2S stress corrosion often show a phenomenon of one gain and the other loss, which makes the manufacture of high-strength H2S stress corrosion resistant oil casing very difficult. Based on this, an embodiment of the present invention provides a corrosion-resistant oil casing, wherein, by mass percentage, the corrosion-resistant oil casing includes the following chemical components:
[0034] C 0.2%~0.3%, Si 0.15%~0.4%, Mn 0.3%~0.7%, Cr 1.9%~2.1%, Mo0.25%~0.45%, Ni 0%~0.25%, Cu 0%~0.25%, V 0%~0.08%, Ti 0.01%~0.03%, Re 0.001%~0.0025%, Al 0.012%~0.02%, Ca 0.012%~0.02%, P 0%~0.015%, S0%~0.005%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0035] In terms of component design, the embodiments of the present invention comprehensively consider multiple requirements of the strength, plasticity, toughness, corrosion resistance, etc. of the oil casing, adopt medium and low C content, add Cr and Mo, V and Ti can be added for microalloying, a small amount of Ni and Cu can be added, rare earth (Re) elements are added, impurities such as P, S, O, H, N and harmful gas elements in the steel are controlled, Al and Si fully deoxidized killed steel is adopted, and the molten steel is subjected to Ca treatment. The chemical composition and content of the corrosion-resistant oil casing are designed by the present invention so that synergistic effects are produced between the elements, and finally the corrosion-resistant oil casing has low cost, high strength, good toughness (toughness is the guarantee of safe service of steel materials) and corrosion resistance. That is, the present invention obtains high corrosion resistance under the premise of ensuring that the oil casing has high strength, plasticity, toughness and low cost. The yield strength level of the corrosion-resistant oil casing can reach the requirements of 80ksi, 95ksi, 110ksi and 125ksi steel grades respectively, the room temperature yield strength is greater than 552-862MPa, the tensile strength is greater than 655-931MPa, the total elongation is greater than or equal to 14%, and the 0°C Charpy V-notch impact toughness is greater than or equal to 90J; according to the NACE TM 0177A method, a 720-hour test in solution A with 85% yield strength stress level (ordinary sulfur-resistant S) and 95% yield strength stress level (super sulfur-resistant SS) does not produce cracks or fractures; in P CO2 ≤0.2MPa、Cl - ≤25g / L, temperature ≤170℃ (i.e., CO2 pressure is less than or equal to 0.2MPa, Cl - Under the environmental conditions of content less than or equal to 25g / L and temperature less than or equal to 170℃), the uniform corrosion rate is less than 0.125mm / a (millimeter / year), which can meet the demand for economical corrosion-resistant oil casing in the development of oil and gas containing H2S and low CO2 content.
[0036] Among them, C is the most important strengthening element. Too low a content is not conducive to improving strength, while too high a content is not conducive to plasticity, toughness and corrosion resistance. Taking all factors into consideration, the C content should be controlled within the range of 0.2% to 0.3%.
[0037] Si is a common element in steel and also acts as a deoxidizer. The Si content should be controlled within the range of 0.15% to 0.4%.
[0038] Mn is mainly used to improve the hardenability of steel, thereby improving the strength of steel, but it has a greater tendency to segregate and is easy to form MnS inclusions with S, which is unfavorable to the plasticity, toughness and corrosion resistance of steel, so it must be strictly controlled. The content of Mn should be controlled within the range of 0.3% to 0.7%.
[0039] Cr is mainly used to improve the hardenability of steel, thereby improving the strength and tempering stability of steel, and at the same time can improve the corrosion resistance of steel, but too high a content will significantly increase the cost. Taking all factors into consideration, the Cr content should be controlled within the range of 1.9% to 2.1%.
[0040] Mo is mainly used to improve the hardenability of steel, thereby improving the strength and tempering stability of steel, and can also improve the corrosion resistance of steel, but too high a content will significantly increase the cost. Taking all factors into consideration, the content of Mo should be controlled within the range of 0.25% to 0.45%. The reasonable matching of the Cr and Mo elements in the present embodiment is conducive to obtaining good corrosion resistance.
[0041] Cu is mainly used to improve the corrosion resistance of steel, and can also improve the hardenability and strength of steel, but too high a content will cause Cu brittleness. Taking all factors into consideration, the Cu content should be controlled within the range of 0% to 0.25%.
[0042] Ni is mainly used to improve the hot brittleness that may be caused by the addition of Cu, and at the same time can improve the hardenability of steel, thereby improving the strength and plasticity of steel. Taking all factors into consideration, the content of Ni should be controlled within the range of 0% to 0.25%.
[0043] V is added to steel to form VC and VN with C and N in the steel, which has the effect of hindering the growth of austenite grains, refining grains, and improving strength and toughness. However, if the content is too high, it will increase the cost and form too much V carbonitride, which will increase brittleness. Taking all factors into consideration, the V content should be controlled within the range of V 0% to 0.08%.
[0044] Ti is added to steel to form TiC and TiN with C and N in the steel, which has the effect of hindering the growth of austenite grains, refining grains, and improving strength and toughness. However, if the content is too high, it will increase the cost and form too much Ti carbonitride, which will increase brittleness. Taking all factors into consideration, the content of Ti should be controlled within the range of 0.01% to 0.03%.
[0045] Ca can improve the properties and morphology of inclusions, thereby improving the plasticity, toughness and corrosion resistance of steel. To ensure the deformation control effect of inclusions, Ca / S>2 should be controlled. Taking all factors into consideration, the content of Ca should be controlled within the range of 0.012% to 0.02%.
[0046] Re has multiple functions of purifying molten steel, refining grains, modifying inclusions, and alloying. Taking all factors into consideration, the content of Re should be controlled within the range of 0.001% to 0.0025%.
[0047] Al is an important deoxidizer. It forms oxides with oxygen to deoxidize. It forms nitrides with nitrogen to partially eliminate the adverse effects of N on plasticity and toughness. It also refines grains and improves strength and plasticity and toughness. To ensure the effect of deoxidation and N control, Al / N>2 is required. Taking all factors into consideration, the Al content should be controlled within the range of 0.012% to 0.02%.
[0048] P is a harmful element that mainly affects the plasticity, toughness and corrosion resistance of steel. The P content should be controlled within the range of 0% to 0.015%.
[0049] S is a harmful element that mainly affects the plasticity, toughness and corrosion resistance of steel. The S content should be controlled within the range of 0% to 0.005%.
[0050] O, H and N are harmful elements, which mainly affect the plasticity, toughness and corrosion resistance of steel. It is advisable to control O+H+N≤0.008%, that is, the total content of O, H and N is less than or equal to 0.008%, among which the N content is controlled in the range of 0% to 0.005%.
[0051] In some embodiments, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0052] C 0.2%~0.25%, Si 0.15%~0.32%, Mn 0.3%~0.68%, Cr 1.9%~2.06%, Mo0.25%~0.35%, Ti 0.01%~0.02%, Re 0.001%~0.002%, Al 0.013%~0.016%, Ca0.012%~0.017%, P 0%~0.012%, S 0%~0.004%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0053] In this embodiment, the corrosion-resistant oil casing can reach 80ksi and 95ksi steel grades respectively, with room temperature yield strength of 609-719MPa, tensile strength of 708-817MPa, total elongation of 26%-31%, 0℃ Charpy V-notch impact toughness of 111-126J, CO2 ≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a. According to the NACE TM 0177A method, no cracks or fractures are generated in the 720-hour test at 85% yield strength stress level and 95% yield strength stress level in solution A. This can meet the demand for economical corrosion-resistant oil casing and tubing for the development of H2S-containing and low CO2-containing oil and gas fields.
[0054] In some embodiments, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0055] C 0.2%~0.22%, Si 0.15%~0.24%, Mn 0.3%~0.47%, Cr 1.9%~1.99%, Mo0.25%~0.3%, Ti 0.01%~0.02%, Re 0.001%~0.002%, Al 0.013%~0.016%, Ca0.012%~0.017%, P 0%~0.012%, S 0%~0.004%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0056] In this embodiment, the corrosion-resistant oil casing can reach 80ksi steel grade, with a yield strength of 609-616MPa, a tensile strength of 708-716MPa, an elongation of 30%-31%, a 0℃ Charpy V-notch impact toughness of 121-126J, and a CO2 ≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a. According to the NACETM 0177A method, no cracks or fractures are generated in the 720-hour test of 85% yield strength stress level and 95% yield strength stress level in solution A. This can meet the demand for economical corrosion-resistant oil casing and tubing for the development of H2S-containing and low-CO2-containing oil and gas fields.
[0057] In some embodiments, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0058] C 0.23%~0.25%, Si 0.29%~0.32%, Mn 0.51%~0.68%, Cr 2.03%~2.06%, Mo 0.32%~0.35%, Ti 0.016%~0.019%, Re 0.0013%~0.0019%, Al 0.013%~0.015%, Ca 0.013%~0.015%, P 0%~0.012%, S 0%~0.003%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0059] In this embodiment, the corrosion-resistant oil casing can reach 95ksi steel grade, with a yield strength of 711-719MPa, a tensile strength of 808-817MPa, an elongation of 26%-27%, a 0℃ Charpy V-notch impact toughness of 111-116J, and a CO2 ≤0.2MPa、Cl -Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a. According to the NACETM 0177A method, no cracks or fractures are generated in the 720-hour test of 85% yield strength stress level and 95% yield strength stress level in solution A. This can meet the demand for economical corrosion-resistant oil casing and tubing for the development of H2S-containing and low-CO2-containing oil and gas fields.
[0060] In some embodiments, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0061] C 0.25%~0.3%, Si 0.31%~0.4%, Mn 0.46%~0.7%, Cr 1.95%~2.1%, Mo0.36%~0.45%, Ni 0.15%~0.25%, Cu 0.15%~0.25%, V 0.03%~0.08%, Ti0.021%~0.03%, Re 0.0016%~0.0025%, Al 0.012%~0.02%, Ca 0.015%~0.02%, P0%~0.012%, S 0%~0.002%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0062] In this embodiment, the corrosion-resistant oil casing can reach 110ksi and 125ksi steel grades, respectively, with a yield strength of 818-927MPa, a tensile strength of 909-1008MPa, an elongation of 21%-24%, a 0°C Charpy V-notch impact toughness of 91-109J, and a CO2 ≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a. According to the NACE TM 0177A method, no cracks or fractures are generated in the 720-hour test at 85% yield strength stress level in solution A. This can meet the demand for economical corrosion-resistant oil casing and tubing for the development of H2S-containing and low-CO2-containing oil and gas fields.
[0063] In some embodiments, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0064] C 0.25%~0.27%, Si 0.31%~0.36%, Mn 0.46%~0.49%, Cr 1.95%~1.99%, Mo 0.36%~0.39%, Ni 0.15%~0.19%, Cu 0.15%~0.21%, V 0.03%~0.05%, Ti0.021%~0.023%, Re 0.0016%~0.0025%, Al 0.012%~0.017%, Ca0.015%~0.019%, P 0%~0.012%, S 0%~0.002%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0065] In this embodiment, the corrosion-resistant oil casing can reach 110ksi steel grade, with a yield strength of 818-826MPa, a tensile strength of 909-918MPa, an elongation of 23%-24%, a 0°C Charpy V-notch impact toughness of 104-109J, and a CO2 ≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a. According to the NACETM 0177A method, no cracks or fractures are generated in the 720-hour test of 85% yield strength stress level and 95% yield strength stress level in solution A. This can meet the demand for economical corrosion-resistant oil casing and tubing for the development of H2S-containing and low-CO2-containing oil and gas fields.
[0066] In some embodiments, the corrosion-resistant oil casing comprises the following chemical components by mass percentage:
[0067] C 0.28%~0.3%, Si 0.35%~0.4%, Mn 0.55%~0.7%, Cr 2.01%~2.1%, Mo0.4%~0.45%, Ni 0.21%~0.25%, Cu 0.22%~0.25%, V 0.06%~0.08%, Ti 0.023%~0.03%, Re 0.002%~0.0023%, Al 0.017%~0.02%, Ca 0.016%~0.02%, P 0%~0.011%, S 0%~0.001%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
[0068] In this embodiment, the corrosion-resistant oil casing can reach 125ksi steel grade, with a yield strength of 920-927MPa, a tensile strength of 1000-1008MPa, an elongation of 21%-22%, a 0°C Charpy V-notch impact toughness of 91-95J, and a CO2≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is less than 0.125mm / a. According to the NACETM 0177A method, no cracks or fractures are generated in the test of 85% yield strength stress level in solution A for 720 hours, which can meet the demand for economical corrosion-resistant oil casing in the development of H2S and low CO2 oil and gas fields.
[0069] In addition to the reasonable design of chemical composition and proportion content, the excellent comprehensive performance of the oil casing and tubing also requires the manufacturing process to affect the final performance of the oil casing and tubing. Different chemical composition designs require the use of different manufacturing processes to enable the oil casing and tubing to exert the best performance. The present invention develops a matching manufacturing process for the chemical composition with the above-mentioned proportion content, mainly through steelmaking (including refining outside the furnace, vacuum degassing), continuous casting, hot perforation, hot rolling in the austenite zone, controlled rolling and controlled cooling, tempering heat treatment, hot straightening and hot sizing, etc., so that the material obtains a fine and uniform tempered troostite microstructure, so as to achieve a reasonable match between the CO2 and H2S corrosion resistance of the oil casing and the strength and plastic toughness. Specifically, an embodiment of the present invention also provides a method for preparing a corrosion-resistant oil casing and tubing, comprising the steps of:
[0070] S1. After batching, smelting and continuous casting of the chemical composition of the corrosion-resistant oil casing according to the embodiment of the present invention, a continuous casting billet is obtained;
[0071] S2, hot piercing and hot rolling the continuous casting billet to obtain a tube billet;
[0072] S3, subjecting the tube blank to tempering heat treatment, heat straightening and heat sizing to obtain the corrosion-resistant oil casing.
[0073] The chemical composition and manufacturing process of the embodiment of the present invention are used in combination to achieve the effects of economy, increased strength, improved toughness, and increased CO2 and H2S corrosion resistance.
[0074] The preparation method of the present invention is aimed at the oil casing with the above chemical composition, obtains the expected organizational structure and performance, gives full play to the performance of the oil casing, has low cost, and the process parameters in the process are easy to control, and the obtained oil casing has stable performance.
[0075] In step S1, in some embodiments, after smelting and continuous casting, the step of obtaining the continuous casting billet specifically includes:
[0076] The raw materials obtained by batching are subjected to oxygen-blown converter smelting, rare earth wire feeding, external refining, vacuum degassing and Si-Ca wire feeding for modification of inclusions to obtain molten steel;
[0077] The molten steel is cast into a rod-shaped continuous casting billet.
[0078] In step S2, in some embodiments, the step of obtaining a tube billet after piercing and hot rolling the continuous casting billet specifically includes:
[0079] The continuous casting billet is heated at 1150-1250° C. for 90-120 min, then hot-pierced at 1145-1200° C., hot-rolled at 880-1150° C. (the hot-rolling deformation is controlled to be 70-80%), and cooled to obtain a tube billet.
[0080] According to the different performance requirements of different steel grades of oil pipes and casings, two methods can be used for heat treatment. In step S3, in some embodiments, the tube blank is subjected to tempering heat treatment, heat straightening and heat sizing to obtain the corrosion-resistant oil casing and casing, which specifically includes:
[0081] For 80ksi and 95ksi steel grade oil casing: the final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed (cooling rate is 15-50°C / s), tempered at 640-700°C for 90-120min and then water cooled (water cooling after tempering to avoid possible temper brittleness); hot straightening and hot sizing are performed at 570-650°C and then water cooled to obtain the corrosion-resistant oil casing;
[0082] For the oil casing of 110ksi and 125ksi steel grades: the final rolling temperature is controlled to be 880-930°C, internal and external water spray quenching is performed (cooling rate is 15-50°C / s), tempering is performed at a temperature of 640-700°C for 90-120min and then water cooling is performed; reheating is performed to 880-930°C, heat preservation is performed for 60-90min, internal and external water spray quenching is performed (cooling rate is 15-50°C / s), tempering is performed at a temperature of 610-650°C for 90-120min and then water cooling is performed; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water cooling is performed to obtain the corrosion-resistant oil casing.
[0083] In this embodiment, a good strengthening effect is obtained by precisely controlling the hot rolling deformation, rolling temperature (especially the final rolling temperature), and cooling rate; direct quenching using the residual heat of rolling reduces the reheating process and can further reduce the production cost (high-strength oil casing generally uses two tempering (quenching + tempering) heat treatments, which has a high production cost). Through hot straightening and hot sizing, the geometric dimensions of the steel pipe meet the requirements, and the residual stress of the oil pipe and casing is effectively controlled to improve the corrosion resistance.
[0084] The method for preparing the corrosion-resistant oil casing also includes the steps of processing API (American Petroleum Institute) standard threads or special threads at the end of the tube blank and performing magnetic particle detection on the threads.
[0085] The following describes it in detail through specific embodiments.
[0086] The chemical compositions of the corrosion-resistant oil pipes and casings used in the following examples are shown in Table 1.
[0087] Table 1. Chemical composition of corrosion-resistant tubing and casing
[0088]
[0089] Note: In each embodiment of Table 1, the chemical composition of the corrosion-resistant oil pipe and casing also includes N, H, O, Fe and inevitable impurities, wherein the N content is 0.005%, the total content of N, H and O is 0.008%, and Fe and inevitable impurities are the remainder.
[0090] Example 1
[0091] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, comprising the following steps:
[0092] Steelmaking: The corrosion-resistant oil pipe and casing of Example 1 are prepared according to the chemical composition shown in Table 1 above, and then subjected to oxygen-blown converter steelmaking, feeding rare earth (Re) wire, refining outside the furnace, vacuum degassing and feeding Si-Ca wire to modify the inclusions in the steel to obtain molten steel.
[0093] Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and soft pressure reduction technology are used to control the segregation in the continuous casting billets.
[0094] Hot piercing and hot rolling: The continuous casting billet is heated in a ring heating furnace at a temperature of 1190±15°C for 120 minutes, and then hot piercing is performed at a temperature of 1170±15°C, followed by hot rolling at a starting temperature of 1150°C and a final rolling temperature of 880°C. The hot rolling deformation is controlled to be 70% to obtain a tube billet;
[0095] Tempering heat treatment, hot straightening and hot sizing: the final rolling temperature is controlled at 880℃, and then the tube blank is subjected to internal and external water spray quenching (cooling rate is 15℃ / s); then tempered at 690±10℃ for 90min, and water cooled after tempering; then hot straightening and hot sizing are carried out at 640±10℃, and then non-destructive testing is carried out on the oil pipe and casing after water cooling; API standard threads are processed at the pipe ends, and magnetic particle testing is carried out on the threads to obtain the oil pipe and casing respectively.
[0096] Example 2
[0097] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, which is different from Embodiment 1 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipe and casing of Embodiment 2 shown in Table 1 above.
[0098] Example 3
[0099] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, which is different from Embodiment 1 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipe and casing of Embodiment 3 shown in Table 1 above.
[0100] Example 4
[0101] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, comprising the following steps:
[0102] Steelmaking: The corrosion-resistant oil pipe and casing of Example 4 are prepared according to the chemical composition shown in Table 1 above, and then subjected to oxygen-blown converter steelmaking, feeding rare earth (Re) wire, refining outside the furnace, vacuum degassing and feeding Si-Ca wire to modify the inclusions in the steel to obtain molten steel.
[0103] Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and soft pressure reduction technology are used to control the segregation in the continuous casting billets.
[0104] Hot piercing and hot rolling: The continuous casting billet is heated in a ring heating furnace at a temperature of 1200±15°C for 120 minutes, and then hot pierced at a temperature of 1180±15°C, and then hot rolled at a starting temperature of 1150°C and a final rolling temperature of 900°C. The hot rolling deformation is controlled to be 70% to obtain a tube billet;
[0105] Tempering heat treatment, hot straightening and hot sizing: the final rolling temperature is controlled at 900℃, and then the tube blank is subjected to internal and external water spray quenching (cooling rate is 15℃ / s); then tempered at 670±10℃ for 100min, and water cooled after tempering; then hot straightening and hot sizing are carried out at 620±10℃, and then non-destructive testing is carried out on the oil pipe and casing after water cooling; API standard threads are processed at the pipe ends, and magnetic particle testing is carried out on the threads to obtain the oil pipe and casing respectively.
[0106] Example 5
[0107] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, which is different from Embodiment 4 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipe and casing of Embodiment 5 shown in Table 1 above.
[0108] Example 6
[0109] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, which is different from Embodiment 4 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipe and casing of Embodiment 6 shown in Table 1 above.
[0110] Example 7
[0111] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, comprising the following steps:
[0112] Steelmaking: The corrosion-resistant oil pipe and casing of Example 7 are prepared according to the chemical composition shown in Table 1 above, and then subjected to oxygen-blown converter steelmaking, feeding of rare earth (Re) wire, refining outside the furnace, vacuum degassing and feeding of Si-Ca wire to modify the inclusions in the steel to obtain molten steel.
[0113] Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and soft pressure reduction technology are used to control the segregation in the continuous casting billets.
[0114] Hot piercing and hot rolling: The continuous casting billet is heated in a ring heating furnace with a heating furnace temperature of 1210±15°C and a heating time of 120min, and then hot piercing is performed at a temperature of 1180±15°C, and then hot rolling is performed with a starting rolling temperature of 1130°C and a final rolling temperature of 900°C. The hot rolling deformation is controlled to be 70% to obtain a tube billet;
[0115] Quenching and tempering heat treatment, hot straightening and hot sizing: the final rolling temperature is controlled at 900℃, and then the tube blank is subjected to internal and external water spray quenching (cooling rate is 15℃ / s); then tempered at 650±10℃ for 110min, and water cooled after tempering; then another quenching and tempering heat treatment is performed, that is, reheated to 900±10℃, kept at temperature for 60min, quenched by internal and external water spray, and then tempered at 640±10℃, the tempering time is 90min, and water cooled after tempering; hot straightening and hot sizing are performed at 600±10℃, and then non-destructive testing is performed on the oil pipe and casing after water cooling; API standard threads are processed at the pipe ends, and magnetic particle testing is performed on the threads to obtain the oil pipe and casing respectively.
[0116] Example 8
[0117] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, which is different from Embodiment 7 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipe and casing of Embodiment 8 shown in Table 1 above.
[0118] Example 9
[0119] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, which is different from Embodiment 7 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipe and casing of Embodiment 9 shown in Table 1 above.
[0120] Example 10
[0121] This embodiment provides a method for preparing a corrosion-resistant oil pipe and casing, comprising the following steps:
[0122] Steelmaking: The corrosion-resistant oil pipe and casing of Example 10 are prepared according to the chemical composition shown in Table 1 above, and then subjected to oxygen-blown converter steelmaking, feeding rare earth (Re) wire, refining outside the furnace, vacuum degassing and feeding Si-Ca wire to modify the inclusions in the steel to obtain molten steel.
[0123] Continuous casting: The molten steel is cast into rod-shaped continuous casting billets. During the continuous casting process, electromagnetic stirring and soft pressure reduction technology are used to control the segregation in the continuous casting billets.
[0124] Hot piercing and hot rolling: The continuous casting billet is heated in a ring heating furnace with a heating furnace temperature of 1170±15°C and a heating time of 120 min, and then hot piercing is performed at a temperature of 1160±15°C, and then hot rolling is performed with a starting rolling temperature of 1110°C and a final rolling temperature of 900°C. The hot rolling deformation is controlled to be 70% to obtain a tube billet;
[0125] Quenching and tempering heat treatment, hot straightening and hot sizing: the final rolling temperature is controlled at 900℃, and then the tube blank is subjected to internal and external water spray quenching (cooling rate is 15℃ / s); then tempering time is 120min at 650±10℃, and water cooling is performed after tempering; then another quenching and tempering heat treatment is performed, that is, reheating to 900±10℃, holding time is 90min, internal and external water spray quenching, and then tempering at 620±10℃, tempering time is 120min, and water cooling is performed after tempering; hot straightening and hot sizing are performed at 580±10℃, and then after water cooling, non-destructive testing is performed on the oil pipe and casing; API standard threads are processed at the pipe end, and magnetic particle testing is performed on the threads to obtain the oil pipe and casing respectively.
[0126] Embodiment 11
[0127] This embodiment provides a method for preparing corrosion-resistant oil pipes and casings, which is different from Embodiment 10 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipes and casings of Embodiment 11 shown in Table 1 above.
[0128] Example 12
[0129] This embodiment provides a method for preparing corrosion-resistant oil pipes and casings, which is different from Embodiment 10 only in that ingredients are prepared according to the chemical composition of the corrosion-resistant oil pipes and casings of Embodiment 12 shown in Table 1 above.
[0130] The corrosion-resistant oil pipes and casings in Examples 1-12 were subjected to yield strength test, tensile strength test, elongation test, 0°C Charpy V-notch impact toughness test, uniform corrosion rate test and NACE TM 0177A method 720-hour hydrogen sulfide stress corrosion test. The results are shown in Table 2 below.
[0131] Table 2. Performance results of corrosion-resistant tubing and casing in Examples 1-12
[0132]
[0133]
[0134] Among them, 2Cr in 2Cr80S means that the Cr content is about 2%, 80 means the yield strength is 80ksi steel grade, S means ordinary sulfur resistance, 2Cr in 2Cr80SS means that the Cr content is about 2%, 80 means the yield strength is 80ksi steel grade, SS means super sulfur resistance. The meanings of other similar writings are similar.
[0135] From the above results, it can be seen that in each embodiment, the yield strength of 80ksi steel grade corrosion-resistant oil pipe and casing (2Cr80S, 2Cr80SS) is 609-616MPa, the tensile strength is 708-716MPa, the elongation is 30%-31%, and the 0°C Charpy V-notch impact toughness is 121-126J.
[0136] 95ksi steel grade corrosion-resistant oil pipes and casing (2Cr95S, 2Cr95SS) have a yield strength of 711-719MPa, a tensile strength of 808-817MPa, an elongation of 26%-27%, and a 0℃ Charpy V-notch impact toughness of 111-116J.
[0137] The yield strength of 110ksi steel grade corrosion-resistant oil pipe and casing (2Cr110S, 2Cr110SS) is 818~826MPa, the tensile strength is 909~918MPa, the elongation is 23%~24%, and the 0℃ Charpy V-notch impact toughness is 104~109J.
[0138] The yield strength of 125ksi steel grade corrosion-resistant oil pipe and casing (2Cr125S) is 920-927MPa, the tensile strength is 1000-1008MPa, the elongation is 21%-22%, and the 0℃ Charpy V-notch impact toughness is 91-95J.
[0139] All the corrosion-resistant oil pipes and casings in the above embodiments 1-12 are CO2 ≤0.2MPa、Cl - Under the conditions of ≤25g / L and temperature ≤170℃, the uniform corrosion rate is <0.125mm / a.
[0140] All the corrosion-resistant tubing and casing in the above Examples 1-9 were subjected to 85% yield strength stress level (ordinary sulfur-resistant S) and 95% yield strength stress level (super sulfur-resistant SS) in solution A for 720 hours according to NACE TM 0177A method without cracks or fractures. All the corrosion-resistant tubing and casing in the above Examples 10-12 were subjected to 85% yield strength stress level (ordinary sulfur-resistant S) in solution A for 720 hours according to NACE TM 0177A method without cracks or fractures.
[0141] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A corrosion-resistant oil casing, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.2%~0.3%, Si 0.15%~0.4%, Mn 0.3%~0.7%, Cr 1.9%~2.1%, Mo 0.25%~0.45%, Ni 0%~0.25%, Cu 0%~0.25%, V 0%~0.08%, Ti 0.01%~0.03%, RE 0.001%~0.0025%, Al0.012%~0.02%, Ca 0.012%~0.02%, P 0%~0.015%, S 0%~0.005%, N 0%~0.005%, O+H+N≤0.008%, the balance is Fe and unavoidable impurities; The method for preparing the corrosion-resistant oil casing comprises the following steps: After batching, smelting and continuous casting according to the chemical composition of the corrosion-resistant oil casing as described above, a continuous casting billet is obtained; The continuous casting billet is subjected to hot piercing and hot continuous rolling to obtain a tube billet; After subjecting the tube blank to tempering heat treatment, heat straightening and heat sizing, the corrosion-resistant oil casing is obtained; After hot piercing and hot rolling the continuous casting billet, the step of obtaining a tube billet specifically includes: The continuous casting billet is heated at a temperature of 1150-1250° C. for 90-120 minutes, then hot-pierced at a temperature of 1145-1200° C., hot-rolled at a temperature of 880-1150° C., and cooled to obtain a tube billet; After the tube blank is subjected to quenching and tempering heat treatment, heat straightening and heat sizing, the steps of obtaining the corrosion-resistant oil casing specifically include: The final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed. After cooling, the steel is tempered at a temperature of 640-700°C for 90-120 minutes and then water-cooled; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water-cooled to obtain the corrosion-resistant oil casing; or, The final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed. After cooling, it is tempered at a temperature of 640-700°C for 90-120 minutes and then water-cooled; it is reheated to 880-930°C, kept warm for 60-90 minutes, internal and external water spray quenching is performed, and after cooling, it is tempered at a temperature of 610-650°C for 90-120 minutes and then water-cooled; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water-cooled to obtain the corrosion-resistant oil casing.
2. The corrosion-resistant oil casing according to claim 1, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.2%~0.25%, Si 0.15%~0.32%, Mn 0.3%~0.68%, Cr 1.9%~2.06%, Mo 0.25%~0.35%, Ti 0.01%~0.02%, RE 0.001%~0.002%, Al 0.013%~0.016%, Ca 0.012%~0.017%, P0%~0.012%, S 0%~0.004%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
3. The corrosion-resistant oil casing according to claim 2, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.2%~0.22%, Si 0.15%~0.24%, Mn 0.3%~0.47%, Cr 1.9%~1.99%, Mo 0.25%~0.3%, Ti 0.01%~0.02%, RE 0.001%~0.002%, Al 0.013%~0.016%, Ca 0.012%~0.017%, P0%~0.012%, S 0%~0.004%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
4. The corrosion-resistant oil casing according to claim 2, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.23%~0.25%, Si 0.29%~0.32%, Mn 0.51%~0.68%, Cr 2.03%~2.06%, Mo 0.32%~0.35%, Ti 0.016%~0.019%, RE 0.0013%~0.0019%, Al 0.013%~0.015%, Ca 0.013%~0.015%, P 0%~0.012%, S 0%~0.003%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
5. The corrosion-resistant oil casing according to claim 1, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.25%~0.3%, Si 0.31%~0.4%, Mn 0.46%~0.7%, Cr 1.95%~2.1%, Mo 0.36%~0.45%, Ni 0.15%~0.25%, Cu 0.15%~0.25%, V 0.03%~0.08%, Ti 0.021%~0.03%, RE0.0016%~0.0025%, Al 0.012%~0.02%, Ca 0.015%~0.02%, P 0%~0.012%, S 0%~0.002%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
6. The corrosion-resistant oil casing according to claim 5, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.25%~0.27%, Si 0.31%~0.36%, Mn 0.46%~0.49%, Cr 1.95%~1.99%, Mo 0.36%~0.39%, Ni 0.15%~0.19%, Cu 0.15%~0.21%, V 0.03%~0.05%, Ti 0.021%~0.023%, RE0.0016%~0.0025%, Al 0.012%~0.017%, Ca 0.015%~0.019%, P 0%~0.012%, S 0%~0.002%, N 0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
7. The corrosion-resistant oil casing according to claim 5, characterized in that: Measured by mass percentage, the corrosion-resistant oil casing includes the following chemical components: C 0.28%~0.3%, Si 0.35%~0.4%, Mn 0.55%~0.7%, Cr 2.01%~2.1%, Mo 0.4%~0.45%, Ni 0.21%~0.25%, Cu 0.22%~0.25%, V 0.06%~0.08%, Ti 0.023%~0.03%, RE0.002%~0.0023%, Al 0.017%~0.02%, Ca 0.016%~0.02%, P 0%~0.011%, S 0%~0.001%, N0%~0.005%, O+H+N≤0.008%, and the balance is Fe and unavoidable impurities.
8. A method for preparing a corrosion-resistant oil casing, characterized in that: Includes steps: After batching, smelting and continuous casting of the chemical composition of the corrosion-resistant oil casing according to any one of claims 1 to 7, a continuous casting billet is obtained; The continuous casting billet is subjected to hot piercing and hot continuous rolling to obtain a tube billet; After subjecting the tube blank to tempering heat treatment, heat straightening and heat sizing, the corrosion-resistant oil casing is obtained; After hot piercing and hot rolling the continuous casting billet, the step of obtaining a tube billet specifically includes: The continuous casting billet is heated at a temperature of 1150-1250° C. for 90-120 minutes, then hot-pierced at a temperature of 1145-1200° C., hot-rolled at a temperature of 880-1150° C., and cooled to obtain a tube billet; After the tube blank is subjected to quenching and tempering heat treatment, heat straightening and heat sizing, the steps of obtaining the corrosion-resistant oil casing specifically include: The final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed. After cooling, the steel is tempered at a temperature of 640-700°C for 90-120 minutes and then water-cooled; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water-cooled to obtain the corrosion-resistant oil casing; or, The final rolling temperature is controlled to be 880-930°C, and internal and external water spray quenching is performed. After cooling, it is tempered at a temperature of 640-700°C for 90-120 minutes and then water-cooled; it is reheated to 880-930°C, kept warm for 60-90 minutes, internal and external water spray quenching is performed, and after cooling, it is tempered at a temperature of 610-650°C for 90-120 minutes and then water-cooled; hot straightening and hot sizing are performed at a temperature of 570-650°C and then water-cooled to obtain the corrosion-resistant oil casing.