A tin-based negative electrode material with composite surface / bulk structure regulation for low-temperature lithium-ion batteries and its application
Patent Information
- Application Number
- CN202311821239.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-12-27
Smart Images

Figure CN117766726B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode material for lithium ion batteries, and more specifically, to a tin-based negative electrode material with a composite surface / bulk structure control for low-temperature lithium ion batteries. The present invention also relates to a method for preparing the negative electrode material. Background Art
[0002] Inside the low-temperature electrode, the electron and ion diffusion kinetics are poor, and the electrode polarization is severe. Low temperature seriously affects the stability and thickness of the SEI film of the negative electrode, resulting in unstable cycles and a sharp drop in performance. However, the theoretical specific capacity of tin oxide negative electrode materials at low temperatures is more than three times that of graphite negative electrode materials, and the lithium insertion voltage is moderate and it is not easy to form dendrites, which is conducive to solving the low-temperature safety problem of commercial graphite negative electrodes. Moreover, tin oxide, as a conversion-alloying negative electrode material, is not affected by the difficulty of low-temperature lithium insertion and is one of the most potential negative electrodes for low-temperature negative electrodes. The main reason is that after tin oxide is converted into tin particles after Li insertion, a transition from β-Sn (tetragonal phase structure, high structural stacking density) to α-Sn (cubic phase structure, low structural stacking density) occurs below 13°C, making it easier for Li to diffuse in α-Sn. However, tin oxide itself has poor conductivity and large volume expansion during lithium insertion / extraction. The poor electron / ion diffusion kinetics at low temperatures have an adverse effect on its low-temperature charging and discharging. Secondly, the volume expansion of the tin oxide negative electrode is large after lithium insertion, resulting in a large volume change during charging and discharging. At the same time, the tin oxide conversion reaction has poor reversibility, and the lithium oxide generated by the conversion reaction is wrapped on the surface of the tin particles, affecting the diffusion of lithium ions, which will further hinder the alloying reaction.
[0003] At present, the mainstream strategies to solve the above problems include regulating the microscopic morphology of tin oxide, element doping and composite with carbon materials. Tin oxide synthesized by morphology control increases the pore structure, thereby increasing the specific surface area, and can show better cycle stability compared with tin oxide before morphology control; secondly, the problem of tin oxide volume expansion can be effectively improved by composite with carbon materials; finally, doping with cations (such as Ti, Ni, etc.) can increase the conductivity of metal oxides and improve the electrochemical properties of tin oxide at low temperatures to a certain extent. However, the current doped elements have basically no improvement on the diffusion ability or kinetics of Li ions at low temperatures, and further exploration and optimization are still needed. Summary of the invention
[0004] In order to improve the working performance of tin oxide electrode materials of lithium ion batteries under low temperature conditions, the present invention provides a tin-based negative electrode material with composite surface / bulk structure control for low temperature lithium ion batteries and a preparation method thereof. The negative electrode material effectively improves the electronic and ionic conductivity of low temperature lithium ion batteries by controlling morphology, doping and compounding.
[0005] The technical solution of the present invention is achieved as follows: a tin-based negative electrode material with composite surface / bulk structure regulation for low-temperature lithium-ion batteries, comprising a doped tin-based negative electrode material and a coating layer coating the doped tin-based negative electrode material; the doped negative electrode material is yttrium-doped nanoflower-shaped tin oxide; the coating layer is a nitrogen-doped carbon layer.
[0006] A method for preparing the above-mentioned tin-based negative electrode material with composite surface / bulk structure control for low-temperature lithium-ion batteries comprises the following steps:
[0007] 1) dispersing yttrium-doped nano-flower-shaped tin oxide in a tris(hydroxymethylamino)methane salt solution, adding dopamine hydrochloride after the dispersion is uniform, and stirring to obtain an intermediate solution;
[0008] 2) washing and drying the intermediate solution obtained in step 1) to obtain an intermediate material;
[0009] 3) heat-treating the intermediate material obtained in step 2) to obtain a tin-based negative electrode material with a composite surface / bulk structure control for use in low-temperature lithium-ion batteries.
[0010] Preferably, the stirring is carried out at room temperature for 20 to 25 hours.
[0011] Preferably, the drying is vacuum drying or freeze drying, wherein vacuum drying is drying at 55-65°C for 10-15 hours, and freeze drying is drying at 0.3mba for 24-36 hours.
[0012] Preferably, the heat treatment process is 1-3°C min -1 The temperature is raised to 200-400°C at a rate of 100°C and calcined for 3-5 hours.
[0013] Preferably, the mass of the dopamine hydrochloride is 95-105 wt.% of the mass of the yttrium-doped flower-shaped tin oxide.
[0014] Preferably, the mass of the tris(hydroxymethyl)aminomethane salt solution is 950-1050wt.% of the mass of the yttrium-doped flower-shaped tin oxide, and the pH value is 8-9.
[0015] Preferably, the method for preparing yttrium-doped nano-flower-shaped tin oxide comprises the following steps:
[0016] 1) Dispersing a tin source, hexadecyltrimethylammonium bromide, sodium citrate dihydrate, and a yttrium source in a mixed solution of ethanol and water in sequence, pouring a sodium hydroxide solution into the mixed solution after uniform dispersion, and continuing to uniformly disperse the mixed solution to obtain a black suspension;
[0017] 2) subjecting the black suspension obtained in step 1) to a hydrothermal reaction, and then sequentially centrifugally washing and drying to obtain an intermediate product;
[0018] 3) heat-treating the intermediate product obtained in step 2) to obtain yttrium-doped nanoflower-shaped tin oxide.
[0019] Preferably, the hydrothermal reaction is carried out in a hydrothermal reactor at 160-200°C for 16-20 hours; the rotation speed of the centrifugal washing is 3000-5000 r min -1 The drying is vacuum drying or freeze drying, wherein vacuum drying is drying at 60-80°C for 11-13 hours, and freeze drying is drying at 0.3mba for 24-36 hours.
[0020] Preferably, the heat treatment process is 1-3°C min -1 The temperature is raised to 400-600°C at a rate of 100°C and calcined for 2-3 hours.
[0021] Preferably, the tin source is one of stannous chloride, stannous octoate, stannous sulfate, and stannous fluoride, or a mixture of any of them.
[0022] Preferably, the yttrium source is one of yttrium nitrate, yttrium carbonate, and yttrium sulfate, or a mixture of any of them.
[0023] Preferably, the mass of the mixed solution of ethanol and water is 3300-3400wt.% of the tin source, and the ethanol concentration is 30-35%; the mass of the hexadecyltrimethylammonium bromide is 160-170wt.% of the tin source; the mass of the sodium citrate dihydrate is 320-330wt.% of the tin source; the mass of the yttrium nitrate hexahydrate is 8-9wt.% of the tin source; the mass fraction of the sodium hydroxide solution is 3-5wt.%, and the mass is 550-560wt.% of the tin source;
[0024] The present invention adopts the above-mentioned technical solution to composite surface / bulk structure control of tin-based negative electrode materials and applies them to low-temperature lithium-ion batteries. The low-temperature performance of lithium-ion batteries is significantly improved, and it also has a significant improvement effect in other temperature ranges. At a low temperature of 0°C, the current density is 100mA g -1 Its first discharge capacity is 805.3 mAh g -1 After 50 cycles, the capacity retention rate is as high as 95%; when the test temperature is reduced to -10 °C, the capacity retention rate is 100mA g -1 After 50 cycles, the capacity retention rate is as high as 91.5%. In addition, when the current density is increased to 400, 800 and 1000 mA g -1 , which still have 529.4, 386.5 and 306.8 mAh g at -10 °C -1The discharge capacity of the battery is 2.3A g / cm2, which shows good low-temperature rate performance. In addition, when the test temperature is 30°C, the discharge capacity of the battery is 1, 5 and 10A g / cm2, which shows good low-temperature rate performance. -1 With up to 892.7, 750.1 and 491.9 mAh g -1 The discharge specific capacity shows good rate performance.
[0025] The advantage of the present invention over the current technology is that the tin-based negative electrode material with a regulated composite surface / bulk structure is applied to low-temperature lithium-ion batteries, and the α-Sn generated by nano-flower-like tin oxide at low temperature is used to improve its low-temperature electrochemical stability. Bulk doping of yttrium atoms reduces the diffusion barrier of lithium ions in tin oxide and accelerates the low-temperature kinetic process; the nitrogen-doped carbon coating layer enhances the surface activity of the tin-based negative electrode, effectively improves the electronic conductivity at low temperatures, inhibits the volume expansion phenomenon of the tin-based material, and improves its cycle stability. At the same time, the lithium ion diffusion rate and cycle stability at room temperature are also excellent. In addition, the material of the present invention has low production cost and simple preparation, and is expected to be applied commercially on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The present invention will be further described in detail below in conjunction with the embodiments in the accompanying drawings, but this does not constitute any limitation to the present invention.
[0027] Figure 1 This is a scanning electron microscope image of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 1 of the present invention.
[0028] Figure 2 This is a comparison diagram of the XRD curves of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 1 of the present invention and the yttrium-doped nanoflower-shaped tin oxide prepared in Comparative Example 1.
[0029] Figure 3 The composite surface / bulk structure-regulated tin-based negative electrode material prepared in Example 1 of the present invention has a current density of 100 mA g at 0°C and -10°C. -1 Cycle performance diagram when .
[0030] Figure 4 The XPS full spectrum of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 2 of the present invention and the XPS high-resolution spectra of Sn 3d, Y 3d, C 1s, O 1s and N1s elements.
[0031] Figure 5 This is a transmission electron micrograph of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 2 of the present invention.
[0032] Figure 6This is a transmission energy spectrum scan distribution diagram of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 2 of the present invention.
[0033] Figure 7 This is a rate performance diagram of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 2 of the present invention at 0°C and -10°C.
[0034] Figure 8 This is a rate performance diagram at 30° C. of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in Example 3 of the present invention and the tin oxide negative electrode material prepared in the comparative example. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully below in conjunction with the accompanying drawings and preferred embodiments, but the protection scope of the present invention is not limited to the following specific embodiments.
[0036] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used below are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0037] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0038] Embodiment 1:
[0039] A tin-based negative electrode material with composite surface / bulk structure regulation for low-temperature lithium-ion batteries is a yttrium-doped nanoflower-shaped tin oxide coated with a nitrogen-doped carbon layer.
[0040] The specific steps of the above composite surface / bulk structure-regulated tin-based negative electrode material are as follows:
[0041] 0.5 g of yttrium-doped nanosheet flower-shaped tin oxide was dispersed in 0.475 L of tris(hydroxymethyl)aminomethane salt solution, and 0.475 g of dopamine hydrochloride was added after uniform dispersion. The solution was stirred for 20 h to obtain an intermediate solution, which was washed and placed in a vacuum drying oven at 55 °C for 15 h to obtain an intermediate material. The intermediate material was dried at 1 °C min -1 The temperature was raised to 200°C at a rate of 200°C and calcined for 5 hours to obtain a tin-based negative electrode material with a composite surface / bulk structure regulation.
[0042] Meanwhile, in this embodiment, the preparation method of yttrium-doped nano-flower-shaped tin oxide comprises the following steps:
[0043] 1) dispersing stannous chloride, hexadecyltrimethylammonium bromide, sodium citrate dihydrate and yttrium nitrate in a mixed solution of ethanol and water in sequence, pouring sodium hydroxide solution into the mixed solution after uniform dispersion, and continuing to disperse uniformly to obtain a black suspension;
[0044] 2) The black suspension obtained in step 1) was kept at 160°C in a hydrothermal kettle for 20 hours, and then heated at a speed of 3000 rmin. -1 The intermediate product was obtained by washing and finally drying at 60°C for 13h.
[0045] 3) The intermediate product obtained in step 2) was heated at 1°C min -1 The temperature was raised to 400°C at a rate of 1.5 °C and calcined for 3 h to obtain yttrium-doped nanoflower-like tin oxide.
[0046] Wherein, the mass of stannous chloride is 10g, the mass of the mixed solution of ethanol and water is 3300wt.% of stannous chloride, and the concentration of ethanol is 30%;
[0047] The mass of the hexadecyltrimethylammonium bromide is 160wt.% of stannous chloride;
[0048] The mass of the sodium citrate dihydrate is 320wt.% of stannous chloride;
[0049] The mass of the yttrium nitrate hexahydrate is 8wt.% of the stannous chloride;
[0050] The mass fraction of the sodium hydroxide solution is 3wt.%, which is 550wt.% of stannous chloride.
[0051] like Figure 1 As shown, it is a scanning electron microscope image of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in this embodiment. Figure 1 It can be seen that the material exhibits a flower-like morphology of nanosheet clusters with a diameter of 200nm.
[0052] The tin-based negative electrode material with composite surface / bulk structure control prepared in this example was subjected to X-ray diffraction test, and its XRD curve is as follows: Figure 2 As shown. By analyzing the XRD data, it can be seen that the peak position of the material is consistent with the standard PDF card of tin oxide, and there is no extra impurity peak of yttrium element.
[0053] The tin-based negative electrode material with composite surface / bulk structure control of this embodiment was made into a lithium-ion battery and its electrochemical performance at low temperature was tested. Figure 3 As shown, at low temperature 0°C, the current density is 100 mA g -1 Its first discharge capacity is 805.3 mAh g -1After 50 cycles, the capacity retention rate is as high as 95%; when the test temperature is reduced to -10 °C, the capacity retention rate is 100mA g -1 After 50 cycles, the capacity retention rate is as high as 91.5%.
[0054] Embodiment 2:
[0055] A tin-based negative electrode material with composite surface / bulk structure regulation for low-temperature lithium-ion batteries is a yttrium-doped nanoflower-shaped tin oxide coated with a nitrogen-doped carbon layer, which has a gap in preparation process compared with other embodiments.
[0056] The specific steps of the above composite surface / bulk structure-regulated tin-based negative electrode material are as follows:
[0057] 0.5 g of yttrium-doped nanosheet flower-like tin oxide was dispersed in 0.5 L of tris(hydroxymethyl)aminomethane salt solution, and 0.5 g of dopamine hydrochloride was added after uniform dispersion. The solution was stirred for 24 h to obtain a brown intermediate solution, which was washed and placed in a vacuum drying oven at 65 °C for 10 h to obtain an intermediate material. The intermediate material was dried at 2 °C min -1 The temperature was raised to 300°C at a rate of 400 °C and calcined for 4 h to obtain a tin-based negative electrode material with a composite surface / bulk structure regulation.
[0058] Meanwhile, in this embodiment, the preparation method of yttrium-doped nano-flower-shaped tin oxide comprises the following steps:
[0059] 1) dispersing stannous octoate, hexadecyltrimethylammonium bromide, sodium citrate dihydrate and yttrium sulfate in a mixed solution of ethanol and water in sequence, pouring sodium hydroxide solution into the mixed solution after uniform dispersion, and continuing to disperse uniformly to obtain a black suspension;
[0060] 2) The black suspension obtained in step 1) was kept at 180°C for 18 hours in a hydrothermal reactor, and then heated at a speed of 4000 rmin. -1 The intermediate product was obtained by washing and finally drying at 80°C for 11h.
[0061] 3) The intermediate product obtained in step 2) was heated at 2°C min -1 The temperature was raised to 500°C at a rate of 2.5°C and calcined for 2.5 hours to obtain yttrium-doped nanoflower-like tin oxide.
[0062] Wherein, the mass of stannous octoate is 10g, the mass of the mixed solution of ethanol and water is 3350wt.% of stannous octoate, and the ethanol concentration is 32%;
[0063] The mass of the hexadecyltrimethylammonium bromide is 165wt.% of stannous octoate;
[0064] The mass of the sodium citrate dihydrate is 325wt.% of stannous octoate;
[0065] The mass of the yttrium sulfate hexahydrate is 8.5wt.% of stannous octoate;
[0066] The mass fraction of the sodium hydroxide solution is 4wt.%, which is 555wt.% of stannous octoate.
[0067] The tin-based negative electrode material with composite surface / bulk structure control prepared in this embodiment was subjected to XPS test. Figure 4 As shown, there are common carbon, nitrogen, tin, oxygen and yttrium peaks, indicating the successful preparation of nitrogen-doped carbon-coated yttrium-doped tin oxide.
[0068] like Figure 5 As shown, it is a high-resolution transmission image of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in this embodiment. The lower right corner is a small Fourier transform image. It can be seen from the figure that the (110) crystal plane spacing is 0.340nm, which is larger than the (110) crystal plane spacing of tin oxide corresponding to the standard PDF card, indicating that yttrium is successfully doped into the tin oxide lattice.
[0069] like Figure 6 As shown, it is the transmission energy spectrum of the tin-based negative electrode material with composite surface / bulk structure regulation prepared in this embodiment, showing five elements Sn, C, Y, N, and O, and the Y element is evenly distributed in the tin oxide, and the nitrogen-doped carbon layer is evenly coated on the surface of the nanoflower cluster.
[0070] The tin-based negative electrode material with composite surface / bulk structure control of this embodiment was made into a lithium-ion battery and its electrochemical performance at low temperature was tested. Figure 7 As shown in Figure 2, when the current density increases to 400, 800, and 1000 mA g -1 , which still have 529.4, 386.5 and 306.8 mAh g at -10 °C -1 The discharge specific capacity shows good low-temperature rate performance.
[0071] Embodiment 3:
[0072] A tin-based negative electrode material with composite surface / bulk structure regulation for low-temperature lithium-ion batteries is a yttrium-doped nanoflower-shaped tin oxide coated with a nitrogen-doped carbon layer, which has a gap in preparation process compared with other embodiments.
[0073] The specific steps of the above composite surface / bulk structure-regulated tin-based negative electrode material are as follows:
[0074] 0.5 g of yttrium-doped nanosheet flower-shaped tin oxide was dispersed in 0.525 L of tris(hydroxymethyl)aminomethane salt solution, and 0.525 g of dopamine hydrochloride was added after uniform dispersion. The solution was stirred for 25 h to obtain an intermediate solution, which was washed and placed in a freeze drying oven under 0.3 mba for 30 h to obtain an intermediate material. The intermediate material was heated at 3 °C min -1 The temperature was raised to 400°C at a rate of 300 °C and calcined for 3 h to obtain a tin-based negative electrode material with a composite surface / bulk structure regulation.
[0075] Meanwhile, in this embodiment, the preparation method of yttrium-doped nano-flower-shaped tin oxide comprises the following steps:
[0076] 1) dispersing stannous sulfate, hexadecyltrimethylammonium bromide, sodium citrate dihydrate and yttrium carbonate in a mixed solution of ethanol and water in sequence, pouring sodium hydroxide solution into the mixed solution after uniform dispersion, and continuing to disperse uniformly to obtain a black suspension;
[0077] 2) The black suspension obtained in step 1) was kept in a hydrothermal kettle at 200°C for 16 h, and then heated at a speed of 5000 rmin -1 The product was washed with , and finally dried at 0.3mba for 28h to obtain an intermediate product;
[0078] 3) The intermediate product obtained in step 2) was heated at 3°C min -1 The temperature was raised to 600°C at a rate of 200 °C and calcined for 2 h to obtain yttrium-doped nanoflower-like tin oxide.
[0079] Wherein, the mass of stannous sulfate is 10g, the mass of the mixed solution of ethanol and water is 3400wt.% of stannous sulfate, and the concentration of ethanol is 35%;
[0080] The mass of the hexadecyltrimethylammonium bromide is 170wt.% of stannous sulfate;
[0081] The mass of the sodium citrate dihydrate is 330wt.% of stannous sulfate;
[0082] The mass of the yttrium carbonate hexahydrate is 9wt.% of stannous sulfate;
[0083] The mass fraction of the sodium hydroxide solution is 5wt.%, which is 560wt.% of stannous sulfate.
[0084] The tin-based negative electrode material with composite surface / bulk structure control of this embodiment was made into a lithium-ion battery and its electrochemical performance was tested at room temperature. Figure 8 As shown, at 30°C, it has a -1 With up to 892.7, 750.1 and 491.9 mAh g -1The discharge specific capacity shows good rate performance.
[0085] Comparative Example:
[0086] The specific steps of the preparation method of yttrium-doped nano-flower-shaped tin oxide are as follows:
[0087] 0.9 g of analytically pure stannous chloride dihydrate, 1.45 g of hexadecyltrimethylammonium bromide, 2.94 g of sodium citrate dihydrate, and 0.07638 g of analytically pure yttrium nitrate hexahydrate were dispersed in a mixed solution of 10 mL of ethanol and 20 mL of deionized water in sequence. After being evenly dispersed, 5 mL of 4.wt% sodium hydroxide solution was poured in. After being evenly dispersed, a yellow suspension was obtained. The suspension was placed in a 100 mL hydrothermal kettle for a hydrothermal reaction at 180 ° C for 18 h, and then heated at a speed of 4000 r min. -1 After centrifugation and washing, the intermediate product was dried overnight at 70 °C in vacuum and then subjected to 3 °C min -1 The temperature is raised to 500°C at a rate of 200°C and calcined for 2 hours to obtain yttrium-doped nanoflower-like tin oxide.
[0088] The yttrium-doped nanoflower-shaped tin oxide of the comparative example was made into a lithium-ion battery and its electrochemical performance was tested. Figure 8 As shown, the current density in the first ten cycles is 0.1A -1 During the cycle, the specific capacity showed an obvious attenuation trend, and then with the increase of current density, it decreased to 10Ag -1 It is basically unable to work under this condition and exhibits poor rate performance.
[0089] The above embodiments are preferred implementation modes of the present invention and are only used to facilitate the description of the present invention. They are not intended to limit the present invention in any form. Any person with ordinary knowledge in the relevant technical field, if they do not depart from the scope of the technical features of the present invention, can make equivalent embodiments by partial changes or modifications to the technical contents disclosed in the present invention, and they still fall within the scope of the technical features of the present invention without departing from the technical features of the present invention.
Claims
1. A tin-based negative electrode material with composite surface / bulk structure control for low-temperature lithium-ion batteries, comprising a doped tin-based negative electrode material and a coating layer coating the doped tin-based negative electrode material, characterized in that: The doped tin-based negative electrode material is nano-flower-shaped tin oxide doped with yttrium atoms, and its diameter is 200-300 nm; the coating layer is a nitrogen-doped carbon layer; The preparation method comprises the following steps: 1) Disperse yttrium-doped nanoflower-like tin oxide in a tris(hydroxymethyl)aminomethane salt solution, add dopamine hydrochloride after the dispersion is uniform, and continue stirring for 20-25 hours to obtain an intermediate solution; 2) washing and drying the intermediate solution obtained in step 1) to obtain an intermediate material, and heat-treating the intermediate material to obtain a tin-based negative electrode material with a composite surface / bulk structure control, wherein the heat treatment process is 1-3 °C min -1 The temperature is raised to 200-400°C at a rate of 100°C and calcined for 3-5 hours; The mass of the dopamine hydrochloride is 95-105 wt. % of the mass of the yttrium-doped nanoflower-shaped tin oxide. The mass of the tris(hydroxymethyl)aminomethane salt solution is 950-1050 wt.% of the mass of the yttrium-doped nanoflower-shaped tin oxide, and the pH value is 8-9; The method for preparing the yttrium-doped nano-flower-shaped tin oxide comprises the following steps: 1) Disperse the tin source, hexadecyltrimethylammonium bromide, sodium citrate dihydrate and yttrium source in a mixed solution of ethanol and water in sequence, pour in the sodium hydroxide solution after uniform dispersion, and continue to disperse uniformly to obtain a white suspension; 2) placing the white suspension obtained in step 1) in a hydrothermal reactor for hydrothermal reaction for 16-20 h, and then centrifugally washing and drying in sequence to obtain an intermediate product, wherein the hydrothermal condition is 160-200° C.; the rotation speed of the centrifugal washing is 3000-5000 r min -1 ; The drying is vacuum drying or freeze drying, wherein vacuum drying is drying at 60-80°C for 11-13 h, and freeze drying is drying at 0.3 mba for 24-36 h; 3) heat-treating the intermediate product obtained in step 2) to obtain yttrium-doped nanoflower-shaped tin oxide, wherein the heat-treatment process is 1-3 °C min -1 The temperature is raised to 400~600℃ at a rate of 200~600℃ and calcined for 2~3 h.
2. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: In the mixed solution of ethanol and water, the mass of the mixed solution is 3300-3400 wt.% of the tin source, and the concentration of ethanol is 30-35%.
3. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: The tin source is one or any combination of stannous chloride, stannous octoate, stannous sulfate and stannous fluoride.
4. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: The yttrium source is one or any combination of yttrium nitrate, yttrium carbonate and yttrium sulfate.
5. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: The mass of the hexadecyltrimethylammonium bromide is 160-170 wt. % of the tin source.
6. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: The mass of the sodium citrate dihydrate is 320-330 wt. % of the tin source.
7. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: The mass of the yttrium source is 8~9 wt. % of the tin source.
8. The tin-based negative electrode material with composite surface / bulk structure control according to claim 1, characterized in that: The mass fraction of the sodium hydroxide solution is 3-5 wt.%, and the mass is 550-560 wt.% of the tin source.