Application of a metal single atom material as a graphite negative electrode additive for lithium-ion batteries and graphite negative electrode for lithium-ion batteries
By using metal single-atom materials as graphite anode additives in lithium-ion batteries, the problem of uneven and unstable lithium deposition in lithium-ion batteries is solved, the safety and life of the battery are significantly improved, and the battery is achieved at low temperatures and high rates. Lithium is uniformly deposited under the conditions, avoiding the generation of lithium dendrites.
Patent Information
- Application Number
- CN202311789583.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-22
AI Technical Summary
The deposition of metallic lithium on the negative electrode of commercial lithium-ion batteries is uneven and unstable, resulting in loss of active lithium capacity and internal short circuit, affecting cycle life and safety performance.
Metal single-atom materials are used as additives for graphite negative electrodes in lithium-ion batteries. Metal single-atom materials are prepared by mixing templates, nitrogen-containing compounds, organic carbon compounds and water-soluble manganese salts, freeze-drying, carbonization and roasting as additives for graphite negative electrodes. Induces uniform deposition of lithium and inhibits the generation of lithium dendrites.
It improves the safety and life of lithium-ion batteries, has a simple preparation process and low cost, and can effectively suppress the generation of lithium dendrites under low temperature and high rate conditions. Only an addition ratio of 1wt% can significantly improve battery performance.
Smart Images

Figure CN117766765B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrode materials, and in particular to an application of a metal single-atom material as a graphite negative electrode additive for a lithium-ion battery and a graphite negative electrode for a lithium-ion battery. Background Art
[0002] With the development and application of lithium-ion batteries in electric vehicles and energy storage, the requirements for the energy density, cycle life and safety performance of lithium-ion batteries are becoming higher and higher. At present, the negative electrode of commercial lithium-ion batteries is mainly graphite-based carbon materials. Due to its low lithium insertion potential, under some harsh charging conditions (low temperature, high rate, etc.), metallic lithium is preferentially deposited on the surface of the graphite negative electrode in the form of dendrites, which is called negative electrode lithium deposition. The deposits of metallic lithium are extremely uneven and unstable, which can lead to loss of active lithium capacity and internal micro-short circuits. It may also puncture the diaphragm to cause internal short circuits and thermal runaway of the battery, which is the main problem affecting the cycle life and safety performance of lithium-ion batteries. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide an application of a metal single atom material as a graphite negative electrode additive for a lithium ion battery and a graphite negative electrode for a lithium ion battery. The present invention uses the metal single atom material as a graphite negative electrode additive for a lithium ion battery, which can induce uniform deposition of lithium precipitated from the graphite negative electrode and inhibit the precipitation of lithium dendrites from the graphite, thereby enhancing the safety and life of the battery.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides an application of a metal single atom material as a graphite negative electrode additive for a lithium ion battery. The preparation method of the metal single atom material comprises the following steps:
[0006] The template, the nitrogen-containing compound, the organic carbon compound, the water-soluble manganese salt and water are mixed and freeze-dried to obtain a precursor;
[0007] The precursor is carbonized and the template is removed in sequence to obtain a carbonized material;
[0008] The carbonized material is calcined to obtain the metal single atom material.
[0009] Preferably, the template agent is sodium chloride; the nitrogen-containing compound is one or more of dicyandiamide, melamine and ammonia; the organic carbon compound is one or more of glucose, melamine, cellulose and citric acid; and the water-soluble manganese salt is manganese acetate tetrahydrate.
[0010] Preferably, the mass ratio of the template, the nitrogen-containing compound, the organic carbon compound and the water-soluble manganese salt is (5000-15000): (500-2000): (300-1200): (0-150), and the mass of the water-soluble manganese salt is not 0; the dosage ratio of the water and the organic carbon compound is 60-80 mL: 0.62 g.
[0011] Preferably, the freeze-drying comprises sequentially performing freezing and drying; the freezing temperature is -50°C and the time is 12 to 48 hours; the drying temperature is -50°C, the pressure is 0.1 to 10 Pa, and the time is 10 to 100 hours.
[0012] Preferably, the carbonization is carried out under a protective atmosphere, the carbonization temperature is 650-795° C., and the time is 1-6 hours.
[0013] Preferably, the calcination is carried out under a protective atmosphere, the calcination temperature is 800 to 1200° C., and the calcination time is 0.5 to 3 hours.
[0014] The present invention provides a lithium-ion battery graphite negative electrode, comprising a current collector and a graphite negative electrode material coated on the surface of the current collector, wherein the graphite negative electrode material comprises graphite, an additive, a binder and a conductive agent, and the additive is a metal single atom material in the application described in the above technical solution.
[0015] Preferably, the mass ratio of the additive to graphite is (0.2-5):100; the mass of the binder and the conductive agent is 1-12.5% of the total mass of the additive and graphite, respectively.
[0016] Preferably, the compaction density of the graphite negative electrode material is 1.4 to 1.6 g / cm 3 .
[0017] The present invention provides a method for preparing a graphite negative electrode for a lithium ion battery according to the above technical solution, comprising the following steps:
[0018] The graphite, additives, binder, conductive agent and organic solvent are mixed to obtain slurry;
[0019] The slurry is coated on the surface of the current collector, dried and then rolled to obtain the lithium ion battery graphite negative electrode.
[0020] The present invention provides an application of a metal single-atom material as a graphite negative electrode additive for lithium-ion batteries. The preparation method of the metal single-atom material comprises the following steps: mixing a template, a nitrogen-containing compound, an organic carbon compound, a water-soluble manganese salt and water, and freeze-drying to obtain a precursor; carbonizing the precursor and removing the template in sequence to obtain a carbonized material; and calcining the carbonized material to obtain the metal single-atom material. The metal single-atom (single-atom manganese) material of the present invention has a good adsorption effect on lithium, can induce the uniform deposition of lithium precipitated from the graphite negative electrode under extreme conditions such as low temperature and high rate, avoids the generation of lithium dendrites, thereby enhancing the safety and life of the battery, and the metal single-atom material has the characteristics of simple preparation process, low synthesis cost, and can be prepared in large quantities. The results of the embodiment show that the metal single-atom material of the present invention is added in a low proportion in the graphite negative electrode, and only 1wt% needs to be added to have an excellent effect of inhibiting the precipitation of lithium dendrites from graphite. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a structural diagram of the metal single atom material of the present invention;
[0022] Figure 2 The spherical aberration electron microscopy photo (HAADF-STEM) and the Fourier transform of synchrotron radiation absorption spectrum (FT-EXAFS) of the metal single atom material prepared in Example 1 are shown in FIG. Figure 2 a is HAADF-STEM, b is FT-EXAFS;
[0023] Figure 3 The SEM images of the graphite pole piece of Example 1 showing the deposition and deintercalation of lithium at different currents are shown below. Figure 3 a~c are SEM images of deposited lithium, d~f are SEM images of deintercalated lithium;
[0024] Figure 4 The SEM images of the graphite pole piece of Example 2 under different currents for lithium deposition and lithium deintercalation are shown in FIG. Figure 4 a~c are SEM images of deposited lithium, d~f are SEM images of deintercalated lithium;
[0025] Figure 5 The SEM images of the graphite pole piece of Example 3 showing the deposition and deintercalation of lithium at different currents are shown in Figure 2. Figure 5 a~c are SEM images of deposited lithium, d~f are SEM images of deintercalated lithium;
[0026] Figure 6 The SEM images of the graphite pole piece of comparative example 1 showing the deposition and deintercalation of lithium at different currents are shown in FIG. Figure 6 a~c are SEM images of deposited lithium, d~f are SEM images of deintercalated lithium;
[0027] Figure 7 The TOF-SIMS of the graphite pole pieces of Example 2 and Comparative Example 1 are shown in Figure 2. Figure 7 a to b correspond to the time-of-flight-secondary ion mass spectra of lithium deposited at 1C current in Example 2 and Comparative Example 1, respectively, and c to d correspond to the time-of-flight-secondary ion mass spectra of lithium deintercalated at 1C current in Example 2 and Comparative Example 1, respectively;
[0028] Figure 8 The following is a bar graph of the residual dead lithium content on the graphite pole pieces of Example 2 and Comparative Example 1 obtained by TGC testing after delithiation. Figure 8 Cells 1 to 2 are graphite pole piece samples of Comparative Example 1, and cells 3 to 4 are graphite pole piece samples of Example 2;
[0029] Fig. 9 The middle is a long cycle performance effect diagram of Example 2 and Comparative Example 1 under high rate (2C) cycle conditions;
[0030] Fig.10 The graphite pole pieces of Example 2 and Comparative Example 1 are compared in terms of lithium dendrite precipitation at low temperatures. Fig.10 a~c are optical photographs and SEM images of the graphite pole piece of comparative example 1, and d~f are optical photographs and SEM images of the graphite pole piece of embodiment 2, respectively. DETAILED DESCRIPTION
[0031] The present invention provides an application of a metal single atom material as a graphite negative electrode additive for a lithium ion battery. The preparation method of the metal single atom material comprises the following steps:
[0032] The template, the nitrogen-containing compound, the organic carbon compound, the water-soluble manganese salt and water are mixed and freeze-dried to obtain a precursor;
[0033] The precursor is carbonized and the template is removed in sequence to obtain a carbonized material;
[0034] The carbonized material is calcined to obtain the metal single atom material.
[0035] In the present invention, the raw materials involved are all commercially available products well known in the art.
[0036] The present invention mixes a template, a nitrogen-containing compound, an organic carbon compound, a water-soluble manganese salt and water, and freeze-dries to obtain a precursor. In the present invention, the template is preferably sodium chloride. In the present invention, the nitrogen-containing compound is preferably one or more of dicyandiamide, melamine and ammonia, and more preferably dicyandiamide. In the present invention, the organic carbon compound is preferably one or more of glucose, melamine, cellulose and citric acid, and more preferably glucose. In the present invention, the water-soluble manganese salt is preferably manganese acetate tetrahydrate, and the water is preferably deionized water.
[0037] In the present invention, the mass ratio of the template, the nitrogen-containing compound, the organic carbon compound and the water-soluble manganese salt is preferably (5000-15000): (500-2000): (300-1200): (0-150), and the mass of the water-soluble manganese salt is not 0, more preferably (8000-9000): (1000-1500): (600-700): (5.5-55), and further preferably 8500: 1200: 620: 15-25. In the present invention, the amount ratio of water to the organic carbon compound is preferably 60-80 mL: 0.62 g, more preferably 70-75 mL: 0.62 g.
[0038] The present invention has no special requirements for the mixing method, and the raw materials can be uniformly mixed using a mixing method well known in the art.
[0039] In the present invention, the freeze drying preferably includes freezing and drying in sequence; the freezing temperature is preferably -50°C, the time is preferably 12 to 48 hours, more preferably 12 to 18 hours; the drying temperature is preferably -50°C, the pressure is preferably 0.1 to 10Pa, more preferably 1 to 5Pa, and the time is preferably 10 to 100 hours, more preferably 48 to 50 hours. In the present invention, the freeze drying achieves uniform dispersion of the raw materials and obtains a homogeneous precursor.
[0040] After obtaining the precursor, the present invention sequentially carbonizes the precursor and removes the template to obtain a carbonized material. In the present invention, the carbonization is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen or argon; the carbonization temperature is preferably 650-795°C, more preferably 750-760°C, the rate of heating from room temperature to the carbonization temperature is preferably 4-5°C / min, and the carbonization time is preferably 1-6h, more preferably 2-4h. In the present invention, the carbonization is preferably carried out in a high-temperature tube furnace. During the carbonization process, the organic carbon compound is coated on the surface of the template crystal to form an ultra-thin spatial three-dimensional open-pored carbon skeleton; the nitrogen atoms produced by the decomposition of the nitrogen-containing compound are anchored on the ultra-thin spatial three-dimensional open-pored carbon skeleton; the metal single atoms produced by the decomposition of the water-soluble manganese salt are also anchored on the ultra-thin spatial three-dimensional open-pored carbon skeleton; at the same time, the metal manganese single atoms and nitrogen atoms anchored on the ultra-thin spatial three-dimensional open-pored carbon skeleton form an MN4 site structure.
[0041] In the present invention, the method for removing the template is preferably: mixing the carbonized product obtained by carbonization with water, performing solid-liquid separation on the obtained liquid, and drying the obtained solid. In the present invention, the water is preferably deionized water, and the present invention does not specifically limit the amount of the water, as long as the template can be completely dissolved, thereby achieving the removal of the template. In the present invention, the method of solid-liquid separation is preferably suction filtration; the present invention does not specifically limit the parameters of the drying, as long as the water can be completely removed.
[0042] After obtaining the carbonized material, the present invention roasts the carbonized material to obtain the metal single atom material. In the present invention, the roasting is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen or argon; the roasting temperature is preferably 800-1200°C, more preferably 900-1000°C, and further preferably 950°C, and the rate of heating from room temperature to the roasting temperature is preferably 4-5°C / min, and the roasting time is preferably 0.5-3h, more preferably 1-1.5h. In the present invention, the roasting can reduce the oxygen content in the carbonized material and improve the conductivity.
[0043] In the present invention, the structure of the metal single atom material is as follows Figure 1 As shown ( Figure 1The magenta color is Mn, the green color is N, and the brown color is C). The metal single atom material has a three-dimensional open-pored structure, which is a single atom configuration of a carbon-based, nitrogen-doped MN4 structure. Specifically, the metal single atom material includes an ultra-thin spatial three-dimensional open-pored carbon skeleton, nitrogen atoms and metal manganese single atoms anchored on the ultra-thin spatial three-dimensional open-pored carbon skeleton; the nitrogen atoms and metal manganese single atoms form an MN4 site structure; the mass of the metal manganese single atom is preferably 0.5-10% of the mass of the ultra-thin spatial three-dimensional open-pored carbon skeleton, and the mass of the nitrogen atom is preferably 9.2-12.2% of the mass of the ultra-thin spatial three-dimensional open-pored carbon skeleton. In the present invention, the element N fills the carbon vacancy defects of the ultra-thin spatial three-dimensional open-pored carbon skeleton, forming NC bonds with the surrounding C, and the metal manganese single atom coordinates with the surrounding N to form an MN4 site structure.
[0044] The present invention uses the metal single atom (single atom manganese) material as a graphite negative electrode additive for lithium-ion batteries, wherein the carbon substrate plays the role of substrate and support for the MN4 site, and MN4 has a good adsorption effect on lithium, and can induce the uniform deposition of lithium precipitated from the graphite negative electrode under extreme conditions such as low temperature and high rate, thereby avoiding the generation of lithium dendrites, thereby enhancing the battery safety and life.
[0045] The present invention provides a lithium-ion battery graphite negative electrode, comprising a current collector and a graphite negative electrode material coated on the surface of the current collector, wherein the graphite negative electrode material comprises graphite, an additive, a binder and a conductive agent, and the additive is a metal single atom material in the application described in the above technical solution.
[0046] The present invention has no special requirements for the current collector, and any current collector well known to those skilled in the art may be used.
[0047] In the present invention, the binder is preferably polyvinylidene fluoride (PVDF), the conductive agent is preferably conductive carbon black, and the conductive carbon black is preferably SuperP. In the present invention, the mass ratio of the additive and graphite is preferably (0.2-5):100, more preferably (0.5-5):100, and further preferably 1:100. The metal single atom material of the present invention is added in a low proportion in the graphite negative electrode, and only 1% is needed to have an excellent effect of inhibiting the precipitation of lithium dendrites from graphite. In the present invention, the mass of the binder and the conductive agent are preferably 1-12.5% of the total mass of the additive and graphite, respectively. In the present invention, the compacted density of the graphite negative electrode material is preferably 1.4-1.6 g / cm 3 .
[0048] The present invention provides a method for preparing a lithium ion battery graphite negative electrode according to the above technical solution, comprising the following steps:
[0049] The graphite, additives, binder, conductive agent and organic solvent are mixed to obtain slurry;
[0050] The slurry is coated on the surface of the current collector, dried and then rolled to obtain the lithium ion battery graphite negative electrode.
[0051] In the present invention, the organic solvent is preferably N-methylpyrrolidone (NMP), and the viscosity of the slurry is preferably 4000-8000 cps. In the present invention, the method of mixing the graphite, additives, binder, conductive agent and organic solvent is preferably: dissolving the binder in the organic solvent to obtain a clear colloidal liquid; dispersing the conductive agent in the colloidal liquid to obtain a mixed colloidal liquid; passing the additive through a 100-mesh sieve and mixing it with graphite, and then dispersing the obtained graphite and additive mixture into the mixed colloidal liquid, and finally adjusting the slurry viscosity to the above range by adding an organic solvent.
[0052] The present invention has no special requirements on the operation methods of coating and rolling, and corresponding methods well known to those skilled in the art can be adopted.
[0053] In order to further illustrate the present invention, the application of a metal single atom material provided by the present invention as a graphite negative electrode for lithium-ion batteries and the graphite negative electrode for lithium-ion batteries are described in detail below in combination with examples, but they should not be understood as limiting the scope of protection of the present invention.
[0054] Example 1
[0055] Preparation of metal single-atom materials: First, sodium chloride (8.5g), dicyandiamide (1.2g), glucose (0.62g), and tetrahydrated manganese acetate (22mg) were dissolved in 75mL of deionized water, then frozen at -50°C for 12h, and then dried at -50°C and 1Pa for 48h to obtain a precursor. Then, the above precursor was placed in a high-temperature tube furnace, heated to 760°C at 4°C / min under an Ar atmosphere, and kept warm for 2h; the resulting product was dispersed in deionized water, filtered and dried to obtain a carbonized material. The carbonized material was then placed in a high-temperature tube furnace, heated to 900°C at 4°C / min under an Ar atmosphere, and kept warm for 1h to obtain a metal (manganese) single-atom material, recorded as SAMn.
[0056] Figure 2 The spherical aberration electron microscopy photo (HAADF-STEM) and the Fourier transform of synchrotron radiation absorption spectrum (FT-EXAFS) of the metal single atom material prepared in Example 1 are shown in FIG. Figure 2 a is HAADF-STEM, b is FT-EXAFS. Figure 2 The white bright spot in a is the Mn single atom, indicating that Mn is dispersed on the carbon substrate in the form of single atoms; Figure 2In b, we can see that the SAMn curve only has a Mn-N peak, but no Mn-Mn peak, which means that Mn and N form a bond and exist in the form of a single atom.
[0057] The SAMn synthesized in Example 1 was sieved (100 mesh), and then mixed with graphite at a mass ratio of 0.5:100, and then pulped. The pulping ratio is binder polyvinylidene fluoride (PVDF): conductive agent (SuperP): graphite and SAMn mixture = 1:1:8, and the solvent is N-methylpyrrolidone (NMP). The specific process is to dissolve PVDF in NMP to obtain a clear colloidal liquid, and then disperse the conductive agent in the colloidal liquid, and finally disperse the graphite and SAMn mixture into it, and finally adjust the slurry viscosity to 5000cps by adding NMP. The slurry is then coated, and the graphite pole piece obtained after coating and drying is rolled (the compaction density is controlled at 1.5g / cm 3 ) to obtain a graphite electrode.
[0058] The graphite pole piece obtained in Example 1 was used to assemble a button cell (CR2025) and perform a graphite||Li half-cell test (the electrolyte was 1M LiPF6 in DEC:DMC:EC=1:1:1Vol%with1%VC). The test conditions were divided into two types: (1) lithium deposition: 10 cycles of constant current charge and discharge, with currents of 0.2C, 0.5C, and 1C (1C=340mAh / g), respectively, and a state of charge (SOC) of 130% (SOC refers to the amount of charge. A normal battery is generally considered fully charged when the SOC is 100%. In order to explore the problem of SAMn inhibiting lithium deposition, the present invention continues to charge when SOC=100%, so that lithium is deposited on the graphite surface, thereby characterizing the induced deposition effect of SAMn on the deposited lithium), and the charging cut-off voltage is 1.5V; finally, discharge once more (SOC is still 130%) to deposit lithium on the graphite surface. (2) Lithium deintercalation: 10 cycles of constant current charge and discharge with currents of 0.2C, 0.5C, and 1C (1C = 340 mAh / g) respectively, with a state of charge (SOC) of 130%, and finally one more discharge (SOC still 130%), followed by lithium deintercalation with a current of 0.1C, with a cut-off voltage of 1.5V.
[0059] Figure 3 The SEM images of the graphite pole piece of Example 1 showing the deposition and deintercalation of lithium at different currents. Figure 3 Figures a to c are SEM images of deposited lithium, indicating that 0.5wt% SAMn addition still produces lithium dendrites; Figure 3 Figures d to f are SEM images of lithium deintercalation, indicating that after 0.5wt% of SAMn is added to release lithium, some dead lithium still remains on the graphite surface.
[0060] Example 2
[0061] The SAMn synthesized in Example 1 was sieved (100 mesh), and then mixed with graphite at a mass ratio of 1:100. After mixing, pulping, coating, and rolling were performed in the same manner as in Example 1 to obtain a graphite electrode (denoted as Gr-SAMn).
[0062] The graphite pole piece obtained in Example 2 was assembled into a button cell (CR2025) and subjected to a graphite||Li half-cell test (the electrolyte was 1M LiPF6 in DEC:DMC:EC=1:1:1Vol% with 1%VC). The test method was the same as that in Example 1.
[0063] Figure 4 These are SEM images of lithium deposition and lithium deintercalation of the graphite pole piece of Example 2 at different currents. Figure 4 Figures a to c are SEM images of deposited lithium, indicating that 1wt% of SAMn added can effectively induce uniform lithium deposition without generating lithium dendrites. Figure 4 Figures d to f are SEM images of lithium deintercalation, indicating that after 1 wt% of SAMn is added to remove lithium, no dead lithium remains on the graphite surface, the graphite surface is neat and clean, and the original morphology of the graphite is maintained.
[0064] Example 3
[0065] The SAMn synthesized in Example 1 was sieved (100 mesh), and then mixed with graphite in a mass ratio of 5:100. After mixing, pulping, coating, and rolling were performed in the same manner as in Example 1 to obtain a graphite pole piece.
[0066] The graphite pole piece obtained in Example 3 was assembled into a button cell (CR2025) and subjected to a graphite||Li half-cell test (the electrolyte was 1M LiPF6 in DEC:DMC:EC=1:1:1Vol% with 1%VC), and the test method was the same as that in Example 1.
[0067] Figure 5 These are SEM images of lithium deposition and lithium deintercalation of the graphite pole piece of Example 3 at different currents. Figure 5 Figures a to c are SEM images of deposited lithium, indicating that 5 wt% of SAMn added can effectively induce uniform lithium deposition without generating lithium dendrites. Figure 5 Figures d to f are SEM images of lithium deintercalation, indicating that after 5 wt% of SAMn is added to remove lithium, due to the strong affinity of SAMn for lithium, more SAMn will cause more lithium to remain on the graphite surface and cannot be deintercalated, but no lithium dendrites appear.
[0068] Comparative Example 1
[0069] The graphite without SAMn addition was slurried, coated and rolled in the same manner as in Example 1 to obtain a graphite electrode (denoted as Gr).
[0070] The graphite pole piece obtained in Comparative Example 1 was assembled into a button cell (CR2025) and subjected to a graphite||Li half-cell test (the electrolyte was 1M LiPF6 in DEC:DMC:EC=1:1:1Vol% with 1%VC), and the test method was the same as that in Example 1.
[0071] Figure 6 The SEM images of the graphite pole piece of comparative example 1 showing the deposition and deintercalation of lithium at different currents. Figure 6 Figures a to c are SEM images of deposited lithium, indicating that excess lithium will precipitate on the graphite surface to form lithium dendrites; Figure 6 Figures d to f are SEM images of lithium deintercalation, indicating that the precipitated lithium cannot be completely removed, resulting in a lot of dead lithium remaining on the graphite surface, especially the appearance of a large number of obvious lithium dendrites.
[0072] Figure 7 Time-of-flight-secondary ion mass spectrometry (TOF-SIMS) of the graphite pole pieces of Example 2 and Comparative Example 1. Figure 7 a to b correspond to the time-of-flight-secondary ion mass spectra of lithium deposited at 1C current in Example 2 and Comparative Example 1, respectively, indicating that the lithium precipitated on the graphite surface can be deposited more evenly after adding SAMn, while the lithium precipitated in Comparative Example 1 is not deposited evenly; Figure 7 Figures c to d correspond to the time-of-flight-secondary ion mass spectra of lithium deintercalation and insertion under 1C current in Example 2 and Comparative Example 1, respectively, indicating that after deintercalation, SAMn can make the precipitated lithium reversibly circulate, and very little dead lithium remains, while a lot of dead lithium remains on the surface of Comparative Example 1.
[0073] The graphite pole pieces of Example 2 and Comparative Example 1 after delithiation were subjected to TGC characterization test, and the content of residual dead lithium on the pole pieces was obtained by calculation. The test results are as follows: Figure 8 As shown, Figure 8 Cells 1-2 are graphite pole piece samples (two parallel samples) of Comparative Example 1, and cells 3-4 are graphite pole piece samples (two parallel samples) of Example 2. It can be seen that the residual dead lithium in Comparative Example 1 is significantly more than that in Example 2 using 1wt% SAMn.
[0074] The graphite pole pieces of Example 2 and Comparative Example 1 were compared for the precipitation of lithium dendrites under high magnification conditions. The test conditions were 25°C, 2C. The test method was: The graphite pole pieces of Example 2 and Comparative Example 1 were used as negative electrodes (size 59*77mm 2 , surface loading 2.8mAh / cm 2 ), the positive electrode is purchased commercial LiNi 0.8Co 0.1 Mn 0.1 O2 pole piece (size 57*75mm 2 , surface loading 2.8mAh / cm 2 ), the two were assembled into a soft pack battery, the electrolyte was 1M LiPF6 in EA:FEC=9:1. The test results are as follows Fig. 9 shown. Fig. 9 The long cycle performance of Example 2 and Comparative Example 1 under high rate (2C) cycle conditions is shown in FIG. It can be seen that the capacity retention rate of Example 2 after 1500 cycles reaches 86.2%, which is 23.0% higher than that of Comparative Example 1. This shows that the addition of SAMn can effectively improve the life of the soft pack battery.
[0075] The graphite pole pieces of Example 2 and Comparative Example 1 were compared for the precipitation of lithium dendrites under low temperature conditions. The test conditions were -30°C, 0.3C. The test method was as follows: the graphite pole pieces of Example 2 and Comparative Example 1 were used as negative electrodes (size 59*77mm 2 , surface loading 2.8mAh / cm 2 ), the positive electrode is purchased commercial LiNi 0.8 Co 0.1 Mn 0.1 O2 pole piece (size 57*75mm 2 , surface loading 2.8mAh / cm 2 ), the two were assembled into a soft pack battery, the electrolyte was 1M LiPF6 in EA:FEC=9:1. The test results are as follows Fig.10 shown. Fig.10 a-c are optical photographs and SEM images of the graphite pole piece of comparative example 1, and d-f are optical photographs and SEM images of the graphite pole piece of embodiment 2. It can be seen that the residual lithium on the pole piece of embodiment 2 is less than that on the graphite pole piece of comparative example 1, and SEM also shows that many lithium dendrites remain on the pole piece of comparative example 1, while lithium dendrites are basically not observed in embodiment 2.
[0076] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A graphite negative electrode for a lithium-ion battery, It is characterized in that The invention comprises a current collector and a graphite negative electrode material coated on the surface of the current collector, wherein the graphite negative electrode material comprises graphite, an additive, a binder and a conductive agent, and the additive is a metal single-atom material; and the preparation method of the metal single-atom material comprises the following steps: The template, the nitrogen-containing compound, the organic carbon compound, the water-soluble manganese salt and water are mixed and freeze-dried to obtain a precursor; The precursor is carbonized and the template is removed in sequence to obtain a carbonized material; calcining the carbonized material to obtain the metal single atom material; The mass ratio of the additive to the graphite is 1:100; the masses of the binder and the conductive agent are 1-12.5% of the total mass of the additive and the graphite respectively.
2. The lithium-ion battery graphite negative electrode according to claim 1, It is characterized in that The template agent is sodium chloride; the nitrogen-containing compound is one or more of dicyandiamide, melamine and ammonia; the organic carbon compound is one or more of glucose, melamine, cellulose and citric acid; and the water-soluble manganese salt is manganese acetate tetrahydrate.
3. The lithium ion battery graphite negative electrode according to claim 1 or 2, It is characterized in that The mass ratio of the template, the nitrogen-containing compound, the organic carbon compound and the water-soluble manganese salt is (5000-15000): (500-2000): (300-1200): (0-150), and the mass of the water-soluble manganese salt is not 0; the dosage ratio of the water and the organic carbon compound is 60-80 mL: 0.62 g.
4. The lithium ion battery graphite negative electrode according to claim 1, It is characterized in that The freeze drying comprises freezing and drying in sequence; the freezing temperature is -50°C and the time is 12 to 48 hours; the drying temperature is -50°C, the pressure is 0.1 to 10 Pa and the time is 10 to 100 hours.
5. The lithium ion battery graphite negative electrode according to claim 1, It is characterized in that The carbonization is carried out under a protective atmosphere, the carbonization temperature is 650-795° C., and the time is 1-6 hours.
6. The lithium-ion battery graphite negative electrode according to claim 1, It is characterized in that The calcination is carried out under a protective atmosphere, the calcination temperature is 800-1200° C., and the calcination time is 0.5-3 h.
7. The lithium-ion battery graphite negative electrode according to claim 1, It is characterized in that The compaction density of the graphite negative electrode material is 1.4-1.6 g / cm 3 .
8. The method for preparing the graphite negative electrode for lithium ion batteries according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The graphite, additives, binder, conductive agent and organic solvent are mixed to obtain slurry; The slurry is coated on the surface of the current collector, dried and then rolled to obtain the lithium ion battery graphite negative electrode.