A method for manufacturing a ceramic substrate based on magnetron sputtering technology

Through the combination of the double-layer target material and the quick-change mechanism, the light sensor is used to monitor the automatic replacement of the target material, which solves the problem of target replacement affecting efficiency in ceramic substrate coating, and achieves an efficient and continuous coating process.

CN117778978BActive Publication Date: 2024-10-11SHANDONG GAOTEWELL ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410019972.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-06
Publication Date
2024-10-11
Estimated Expiration
2044-01-06

AI Technical Summary

Technical Problem

During the coating process of ceramic substrates, when the target material needs to be replaced, the sputtering process must be interrupted and the vacuum environment destroyed, affecting the coating efficiency.

Method used

It adopts a double-layer target design, equipped with a hidden spare target and a quick-change mechanism. The target consumption is monitored through a light sensor, and the target replacement is automatically completed to avoid opening the coating machine and maintain the continuity of the sputtering process.

Benefits of technology

It achieves fast and efficient target replacement, reduces the waste of argon gas and the impact on coating efficiency, and improves the continuity and efficiency of metal film plating on ceramic substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117778978B_ABST
    Figure CN117778978B_ABST
Patent Text Reader

Abstract

The present invention relates to a ceramic substrate manufacturing method based on magnetron sputtering technology applied in the field of ceramic substrate coating technology. Through the setting of a double-layer target material, a hidden spare target material is provided. When replacement is needed during the sputtering process, there is no need to open the coating machine. Through a quick-change mechanism, the external target piece and the internal target piece can be automatically and quickly replaced when the coating machine is turned off, so that the sputtering process does not need to be interrupted, or the target material can be replaced with only a short interruption time, thereby achieving the effect of improving efficiency. Compared with the prior art, there is no need to re-create an argon atmosphere, which can effectively reduce the waste of argon gas and greatly reduce the impact on the efficiency of metal film coating on the ceramic substrate. In addition, with the setting of a target material monitoring component, the double-layer target material can be monitored, which is convenient for timely replacement of the external target piece and the internal target piece, thereby effectively maintaining the efficient coating of the ceramic substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ceramic substrate manufacturing method, in particular to a ceramic substrate manufacturing method based on magnetron sputtering technology applied in the field of ceramic substrate coating technology. Background Art

[0002] Magnetron sputtering is a type of physical vapor deposition. The general sputtering method can be used to prepare multiple materials such as metals, semiconductors, insulators, etc., and has the advantages of simple equipment, easy control, large coating area and strong adhesion. Magnetron sputtering introduces a magnetic field on the surface of the target cathode and uses the magnetic field to constrain charged particles to increase the plasma density and increase the sputtering rate, so that the sputtered target material is deposited on the surface of the ceramic substrate to form a copper metal film layer.

[0003] Since the target material is a consumable, there is a need to replace the target material during the batch manufacturing process of ceramic substrate surface coating. However, when the target material needs to be replaced during the coating process, the sputtering coating process needs to be interrupted, the magnetron sputtering coating machine needs to be started, and then the target material needs to be replaced. This method not only interrupts the sputtering process for a long time, but also destroys the vacuum environment in the coating machine. When coating again subsequently, it is necessary to repeatedly create an argon environment, which seriously affects the efficiency of metal film coating on the ceramic substrate surface. Summary of the invention

[0004] In view of the above-mentioned prior art, the technical problem to be solved by the present invention is that during the coating process, when the target material needs to be replaced, the coating equipment must be opened for replacement, which affects the coating efficiency.

[0005] In order to solve the above problems, the present invention provides a method for manufacturing a ceramic substrate based on magnetron sputtering technology, comprising the following steps:

[0006] S1. Firstly, the ceramic substrate is ultrasonically cleaned and dried, and then the dried ceramic substrate is placed in a magnetron sputtering coating machine;

[0007] S2. Then, the air is evacuated from the coating machine and argon gas is introduced to maintain a low-pressure argon atmosphere in the coating machine. Then, the coating power supply is started to start the magnetron sputtering coating process. The magnetic plate array generates magnetic lines of force that hit the double-layer target material, so that the metal atoms of the double-layer target material are sputtered onto the ceramic substrate and accumulated to form a metal film.

[0008] S3. When the double-layer target material is consumed too much and needs to be replaced during magnetron sputtering, the coating power supply is temporarily turned off to cut off the power to the magnetic plate array. At this time, the double-layer target material is replaced by the quick-change mechanism, and the position of the consumed target material and the hidden spare target material is changed to expose the hidden spare target material directly, so that the sputtering process continues until the metal layer reaches the target thickness.

[0009] In the above-mentioned ceramic substrate manufacturing method based on magnetron sputtering technology, a double-layer target material is set up, which has its own hidden spare target material. When replacement is needed, the target material can be quickly replaced without opening the coating machine, so that the sputtering process does not need to be interrupted, or the target material can be replaced with only a short interruption time, thereby achieving the effect of improving efficiency.

[0010] As a further improvement of the present application, the double-layer target material includes a target rotating cylinder, a plurality of compensation belts respectively fixedly connected to the outer ends of the target rotating cylinder, and a plurality of double-layer target plates respectively located between two adjacent compensation belts. The left and right ends of the target rotating cylinder are fixedly connected with a rotating rod, the rotating rod is installed in the coating machine through an electric rotating shaft, and a quick-changing mechanism is provided outside the rotating rod.

[0011] As a further improvement of the present application, a plurality of compensation belts are distributed in a ring array, and a plurality of double-layer target sheets and a plurality of compensation belts form a complete tubular structure.

[0012] As a further improvement of the present application, the two surfaces of the double-layer target sheet contacting the compensation belt are parallel to each other, including a partition plate and an externally visible target sheet and an internally invisible target sheet respectively clamped on the two end surfaces of the partition plate, and the externally visible target sheet faces outward.

[0013] As a further improvement of the present application, the quick-changing mechanism includes two reducing ring groups respectively located on both sides of the target-carrying rotating cylinder, the reducing ring groups include a plurality of target arc blocks and a plurality of electric push rods respectively installed between the target arc blocks and the rotating rods, the extended ends of the electric push rods are fixed to the target arc blocks, and the middle parts of both ends of the double-layer target piece are respectively connected to the two opposite target arc blocks on the two reducing ring groups through electric rotating shafts.

[0014] As a further improvement of the present application, a target material monitoring assembly is installed on one of the compensation belts, and the target material monitoring assembly includes two light sensors respectively located on both sides of the dividing plate. The light sensor is embedded in the compensation belt, and the surface of the light sensor is flush with the inner wall of the compensation belt.

[0015] As a further improvement of the present application, in step S3, the specific steps of target material exchange are:

[0016] S31. When magnetron sputtering coating is performed on the ceramic substrate, the light sensor monitors the light change in real time. When the external target sheet located on the outside is consumed and the light sensor is exposed, the light sensor receives a light signal.

[0017] S32. After receiving the light signal, the coating machine controls the coating power supply to be turned off, and at the same time controls the electric push rod to extend, thereby pushing the arc block with the target to move outward, and the arc block with the target drives the double-layer target sheet to move outward until it is completely separated from the compensation belt;

[0018] S33. Finally, the coating machine controls the electric shaft on the compensation belt to rotate 180° to achieve the replacement of the visible target and the hidden target. At the same time, the electric push rod is controlled to shorten to reset the target arc block, thus completing the closed replacement of the target material.

[0019] As another improvement of the present application, a target material monitoring assembly is installed on the partition plate, and the target material monitoring assembly includes two groups of light sensor matrices respectively located on two end surfaces of the partition plate, and the light sensor matrix includes a plurality of light sensors distributed in a rectangular array.

[0020] In summary, through the setting of a double-layer target material, a hidden spare target material is provided. When it needs to be replaced during the sputtering process, there is no need to open the coating machine. The quick-changing mechanism can automatically and quickly replace the external target and the internal target when the coating machine is turned off, so that the sputtering process does not need to be interrupted, or the target material can be replaced with only a short interruption time, thereby achieving the effect of improving efficiency. Compared with the existing technology, there is no need to re-create the argon atmosphere, which can effectively reduce the waste of argon and greatly reduce the impact on the efficiency of metal film coating on ceramic substrates. In addition, with the setting of the target material monitoring component, the double-layer target material can be monitored, which is convenient for timely replacement of the external target and the internal target, thereby effectively maintaining the efficient coating of the ceramic substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of a coating machine in the first embodiment of the present application;

[0022] Figure 2 This is a schematic radial cross-sectional view of a double-layer target material in a magnetron sputtering process according to a first embodiment of the present application;

[0023] Figure 3 A schematic diagram of a transverse cross section of a double-layer target material according to a first embodiment of the present application;

[0024] Figure 4 This is a schematic diagram of a double-layer target sheet according to the first embodiment of the present application;

[0025] Figure 5 A three-dimensional diagram of a double-layer target material according to the first embodiment of the present application;

[0026] Figure 6 This is an exploded view of a double-layer target material according to the first embodiment of the present application;

[0027] Figure 7 This is a diagram showing changes of the visible target piece and the hidden target piece of the double-layer target piece during the transposition process in the first embodiment of the present application;

[0028] Figure 8 A three-dimensional diagram of a double-layer target sheet according to the first embodiment of the present application;

[0029] Fig. 9 This is a schematic diagram of a target monitoring assembly on a dividing plate in a second embodiment of the present application.

[0030] Description of the numbers in the figure:

[0031] 1 double-layer target material, 11 target-carrying rotating drum, 12 double-layer target piece, 121 external target piece, 122 dividing plate, 123 internal target piece, 13 target arc block, 14 compensation belt, 101 rotating rod, 102 electric push rod. DETAILED DESCRIPTION

[0032] Two implementation modes of the present application are described in detail below with reference to the accompanying drawings.

[0033] The first implementation method:

[0034] Figure 1 As shown, a in the figure represents a ceramic substrate, a method for manufacturing a ceramic substrate based on magnetron sputtering technology, comprising the following steps:

[0035] S1. Firstly, the ceramic substrate is ultrasonically cleaned and dried, and then the dried ceramic substrate is placed in a magnetron sputtering coating machine;

[0036] S2, such as Figure 2 In the figure, b represents the magnetic plate array, and c represents the formed metal film. Then, the air is evacuated from the coating machine and argon gas is introduced to maintain a low-pressure argon atmosphere in the coating machine. Then, the coating power supply is started to start the magnetron sputtering coating process. The magnetic plate array generates magnetic lines of force, which hit the double-layer target material 1, so that the metal atoms of the double-layer target material 1 are sputtered onto the ceramic substrate and accumulated to form a metal film.

[0037] S3. When the double-layer target material 1 is consumed too much and needs to be replaced during the magnetron sputtering process, the coating power supply is temporarily turned off to cut off the power to the magnetic plate array. At this time, the double-layer target material 1 is replaced by the quick-changing mechanism, and the position of the consumed target material and the hidden spare target material is changed to expose the hidden spare target material directly, so that the sputtering process continues until the metal layer reaches the target thickness.

[0038] like Figure 3 The double-layer target material 1 includes a target rotating drum 11, a plurality of compensation belts 14 respectively fixedly connected to the outer ends of the target rotating drum 11, and a plurality of double-layer target pieces 12 respectively located between two adjacent compensation belts 14. The left and right ends of the target rotating drum 11 are fixedly connected with a rotating rod 101, and the rotating rod 101 is installed in the coating machine through an electric rotating shaft. A quick-changing mechanism is arranged outside the rotating rod 101. The quick-changing mechanism can control the outer end surface of the double-layer target piece 12 to change without opening the coating machine, thereby realizing the closed replacement of the target material, effectively reducing the influence of replacing the target material on the coating efficiency during the coating process of the ceramic substrate.

[0039] like Figure 4 The double-layer target plate 12 includes a partition plate 122 and an external target plate 121 and an internal target plate 123 respectively clamped on the two end surfaces of the partition plate 122, the external target plate 121 faces outward, and the two surfaces of the double-layer target plate 12 in contact with the compensation belt 14 are parallel to each other. This arrangement fixes the spacing between two adjacent compensation belts 14, and there is no situation where the outer side is larger and the inner side is smaller. It effectively ensures that before and after the external target plate 121 and the internal target plate 123 are replaced, the double-layer target plate 12 can maintain stable contact with the compensation belt 14, thereby effectively ensuring the stable progress of the magnetron sputtering process.

[0040] like Figure 5-6 , multiple compensation belts 14 are distributed in a ring array, multiple double-layer target plates 12 and multiple compensation belts 14 form a complete tubular structure, the compensation belts 14 are mainly used to correct and compensate the double-layer target plates 12, when the two end surfaces of the double-layer target plates 12 in contact with the compensation belts 14 are flush with each other, the multiple double-layer target plates 12 cannot form a complete tubular structure, under the action of the compensation belts 14, it is not easy to have gaps between the multiple double-layer target plates 12.

[0041] like Figure 6-7 The quick-change mechanism includes two reducer ring groups located on both sides of the target-carrying rotating drum 11, the reducer ring group includes a plurality of target arc blocks 13 and a plurality of electric push rods 102 respectively installed between the target arc blocks 13 and the rotating rod 101, and the extended end of the electric push rod 102 is fixed to the target arc block 13. Figure 8 , and the middle parts of both ends of the double-layer target piece 12 are connected to the two opposite target arc blocks 13 on the two reducing ring groups through electric rotating shafts. The multiple target arc blocks 13 on the two reducing ring groups correspond to each other one by one. The two corresponding target arc blocks 13 can control the position change of the double-layer target piece 12 during the diameter change process through the extension and shortening of the electric push rod 102, and can bring the double-layer target piece 12 away from the space restricted by the two compensation belts 14, thereby rotating and reversing, and realizing closed automatic replacement of the target material.

[0042] A target material monitoring assembly is installed on one of the compensation belts 14. The target material monitoring assembly includes two light sensors located on both sides of the dividing plate 122. The light sensor is embedded in the compensation belt 14, and the surface of the light sensor is flush with the inner wall of the compensation belt 14. When the target material is consumed, the light sensor can monitor the change of light, and the coating machine automatically replaces the target material according to this phenomenon.

[0043] It is worth noting that the distance between the photosensitive end of the light sensor and the dividing plate 122 does not exceed 10 mm, which effectively ensures that the light sensor can receive the signal of light change before the external target piece 121 or the internal target piece 123 is about to be consumed, so as to facilitate timely and rapid replacement of the external target piece 121 or the internal target piece 123 so that the internal target piece 123 faces outward so that the coating process on the surface of the ceramic substrate can proceed smoothly.

[0044] In step S3, the specific steps of target material exchange are:

[0045] S31, when the ceramic substrate is subjected to magnetron sputtering coating, the light sensor monitors the light change in real time, and when the external target sheet 121 located on the outside is consumed to expose the light sensor, the light sensor receives the light signal;

[0046] S32, after receiving the light signal, the coating machine controls the coating power to be turned off, and at the same time controls the electric push rod 102 to extend, thereby pushing the target arc block 13 to move outward, and the target arc block 13 drives the double-layer target sheet 12 to move outward until it is completely separated from the compensation belt 14;

[0047] S33, such as Figure 8 Finally, the coating machine controls the electric shaft on the compensation belt 14 to rotate 180° to achieve the replacement of the visible target piece 121 and the hidden target piece 123, and at the same time controls the electric push rod 102 to shorten the target arc block 13 to reset, completing the closed replacement of the target material.

[0048] In summary, through the setting of the double-layer target material 1, a hidden spare target material is provided. When it needs to be replaced during the sputtering process, there is no need to open the coating machine. Through the quick-changing mechanism, the external target piece 121 and the internal target piece 123 can be automatically and quickly replaced when the coating machine is turned off, so that the sputtering process does not need to be interrupted, or only a short interruption time is required to achieve the target material replacement, thereby achieving the effect of improving efficiency. Compared with the prior art, there is no need to re-create the argon atmosphere, which can effectively reduce the waste of argon gas and greatly reduce the impact on the efficiency of metal film coating on ceramic substrates. In addition, with the setting of the target material monitoring component, the double-layer target material can be monitored, which is convenient for timely replacement of the external target piece and the internal target piece, thereby effectively maintaining the efficient coating of the ceramic substrate.

[0049] The second implementation method:

[0050] This embodiment is based on the first embodiment, and changes the setting method of the target monitoring component, and the rest of the parts are consistent with the first embodiment.

[0051] like Fig. 9In the figure, d represents a light sensor. A target material monitoring assembly is installed on the partition plate 122. The target material monitoring assembly includes two groups of light sensor matrices respectively located on the two end surfaces of the partition plate 122. The light sensor matrix includes a plurality of light sensors distributed in a rectangular array. As the magnetron sputtering process proceeds, the externally visible target piece 121 facing outward is gradually consumed. When the local target piece 121 is consumed, the nearby light sensor can receive the change of the light signal. At this time, the signal can be fed back to the coating machine, so that the coating machine controls the quick-changing mechanism to replace the externally visible target piece 121 and the internally hidden target piece 123, so that the internally hidden target piece 123 faces outward, so as to achieve the effect of replacing the target material without opening the coating machine, so that the coating of the ceramic substrate can be carried out continuously, and the influence on the coating efficiency of the ceramic substrate is effectively reduced.

[0052] In view of current practical needs, the above-mentioned implementation mode adopted in this application is not limited to the scope of protection. Various changes made within the knowledge scope of technical personnel in this field without departing from the concept of this application still fall within the scope of protection of the present invention.

Claims

1. A method for manufacturing a ceramic substrate based on magnetron sputtering technology, characterized in that: The following steps are involved: S1. Firstly, the ceramic substrate is ultrasonically cleaned and dried, and then the dried ceramic substrate is placed in a magnetron sputtering coating machine; S2, then the air is evacuated from the coating machine and argon gas is introduced to maintain a low-pressure argon atmosphere in the coating machine, and then the coating power supply is started to start the magnetron sputtering coating process, the magnetic plate array generates magnetic lines of force, which impact the double-layer target material (1), so that the metal atoms of the double-layer target material (1) are sputtered onto the ceramic substrate and accumulated to form a metal film; S3. When the double-layer target material (1) is consumed excessively during magnetron sputtering and needs to be replaced, the coating power supply is temporarily turned off to cut off the power supply to the magnetic plate array. At this time, the double-layer target material (1) is replaced by the quick-change mechanism, and the positions of the consumed target material and the hidden spare target material are changed so that the hidden spare target material is directly exposed, so that the sputtering process is continued until the metal layer reaches the target thickness; The double-layer target material (1) comprises a target-carrying rotating drum (11), a plurality of compensation belts (14) respectively fixedly connected to the outer ends of the target-carrying rotating drum (11), and a plurality of double-layer target pieces (12) respectively located between two adjacent compensation belts (14). The left and right ends of the target-carrying rotating drum (11) are both fixedly connected to a rotating rod (101). The rotating rod (101) is installed in a coating machine via an electric rotating shaft. A quick-change mechanism is provided outside the rotating rod (101). Two surfaces of the double-layer target piece (12) in contact with the compensation belts (14) are parallel to each other. The double-layer target piece (12) comprises a partition plate (122) and two portions respectively clamped to the partition plate (122). 122) externally visible target pieces (121) and internally invisible target pieces (123) on two end surfaces, the externally visible target piece (121) facing outward, the quick-change mechanism comprising two diameter-changing ring groups respectively located on both sides of the target-carrying rotating cylinder (11), the diameter-changing ring group comprising a plurality of target arc blocks (13) and a plurality of electric push rods (102) respectively installed between the target arc blocks (13) and the rotating rod (101), the extended ends of the electric push rods (102) being fixed to the target arc blocks (13), and the middle parts of both ends of the double-layer target piece (12) are respectively connected to the two opposite target arc blocks (13) on the two diameter-changing ring groups through electric rotating shafts; The plurality of compensation belts (14) are distributed in a ring array, and the plurality of double-layer target sheets (12) and the plurality of compensation belts (14) form a complete tubular structure; In S3, the specific steps of target material exchange are: S31, when magnetron sputtering coating is performed on the ceramic substrate, the light sensor monitors the light change in real time, and when the external target sheet (121) located on the outside is consumed to expose the light sensor, the light sensor receives a light signal; S32, after receiving the light signal, the coating machine controls the coating power supply to be turned off, and at the same time controls the electric push rod (102) to extend, thereby pushing the target arc block (13) to move outward, and the target arc block (13) drives the double-layer target sheet (12) to move outward until it is completely separated from the compensation belt (14); S33, finally the coating machine controls the electric rotating shaft on the compensation belt (14) to rotate 180 degrees, so as to achieve the replacement of the visible target sheet (121) and the hidden target sheet (123), and at the same time controls the electric push rod (102) to shorten so as to reset the target arc block (13), thereby completing the closed replacement of the target material.

2. The method for manufacturing a ceramic substrate based on magnetron sputtering technology according to claim 1, characterized in that: A target material monitoring assembly is installed on one of the compensation belts (14), the target material monitoring assembly comprising two light sensors respectively located on both sides of the dividing plate (122), the light sensors are embedded in the compensation belt (14), and the surface of the light sensor is flush with the inner wall of the compensation belt (14).

3. The method for manufacturing a ceramic substrate based on magnetron sputtering technology according to claim 1, characterized in that: A target material monitoring component is installed on the partition plate (122), and the target material monitoring component comprises two groups of light sensor matrices respectively located on two end surfaces of the partition plate (122), and the light sensor matrix comprises a plurality of light sensors distributed in a rectangular array.