A microwave absorbing material, its preparation method and application

By designing a hollow composite microsphere structure and combining it with a heterogeneous structure of magnetic and non-magnetic metal layers, the density and reflection problems of metal absorbing materials are solved, achieving a balance between low density, high compressive strength, and excellent wave absorption performance, making it suitable for multiple electromagnetic wave absorption application scenarios.

CN117794204BActive Publication Date: 2026-11-10TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211150187.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2026-11-10
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

The high density and continuous film structure of metallic absorbing materials make them prone to reflection during electromagnetic wave absorption, which makes it impossible to effectively utilize their loss capacity and affects the balance between impedance matching and loss capacity.

Method used

A hollow composite microsphere structure is adopted, including hollow silicate glass microspheres, magnetic metal layers and non-magnetic metal layers, forming a heterogeneous structure. The functionality is regulated by controlling the composition and structural design of the metal layers. The magnetic metal layers are composed of mutually isolated magnetic metal regions, and the non-magnetic metal is embedded in the magnetic metal regions to form a heterogeneous structure.

Benefits of technology

It achieves a balance between low density, high compressive strength, and excellent wave absorption performance, effectively absorbing electromagnetic waves and controlling electromagnetic wave reflection loss. It is suitable for military stealth, electromagnetic radiation protection, and building wave absorbing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117794204B_ABST
    Figure CN117794204B_ABST
Patent Text Reader

Abstract

This invention discloses a microwave absorbing material, which is a hollow composite microsphere. Its structure includes: hollow silicate glass microspheres; a magnetic metal layer on the surface of the silicate glass microspheres, the magnetic metal layer being composed of several physically isolated magnetic metal regions; and a non-magnetic metal layer on the magnetic metal layer, the non-magnetic metal layer being composed of non-magnetic metal bonded to at least some of the magnetic metal regions. This microwave absorbing material exhibits excellent compressive strength and microwave absorption properties. This invention also discloses a method for preparing this microwave absorbing material and its applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of microwave absorbing materials technology. More specifically, it relates to a microwave absorbing material, its preparation method, and its applications. Background Technology

[0002] With the rapid development of electronic and communication technologies, electromagnetic waves have been widely used in production and daily life. However, the widespread presence of electromagnetic waves poses a significant threat to the precise operation of equipment and the health of living organisms. To reduce the adverse effects of these electromagnetic waves, electromagnetic wave absorbing materials (wave-absorbing materials) and shielding materials have emerged. Electromagnetic wave absorbing materials based on absorption mechanisms have attracted much attention because they can avoid secondary pollution caused by repeated reflections of electromagnetic waves. To date, numerous materials with conductive, dielectric, and magnetic properties have been designed and developed for use as electromagnetic wave absorbing materials. Among them, metallic materials have been favored by researchers and developers of wave-absorbing materials due to their wide availability and excellent performance. First, the conductivity of metallic materials can be adjusted over a wide range through alloying or morphological manipulation, facilitating the balance between impedance matching and conductivity loss. Second, some metallic materials possess both conductive and magnetic properties, enabling a dual electromagnetic wave loss mechanism. Third, metallic materials can be easily micro / nanosized and their microstructure and composition controlled through bottom-up reduction or top-down pulverization, making it possible to study the structure-property relationships of wave-absorbing materials and to develop and regulate the performance of novel wave-absorbing materials.

[0003] However, compared to other types of absorbing materials, such as ceramics, ferrites, oxides, carbon materials, and conductive polymers, the high density of metallic absorbing materials limits their application range. Furthermore, for conventionally formed continuous film-like thin-shell metal structures, this continuous film structure helps form a continuous macroscopic conductive network, thereby improving performance in metal-based conductive materials or electromagnetic shielding materials. However, for electromagnetic wave absorbing materials, the easily formed conductive network and excessively high conductivity are detrimental to electromagnetic matching design, causing a large amount of incident electromagnetic waves to be reflected at the surface, preventing the effective dissipation of electromagnetic waves. Summary of the Invention

[0004] Based on the above problems, the purpose of this invention is to provide a microwave absorbing material, its preparation method and application, so as to at least improve the problem of effectively balancing the impedance matching and loss capability of the microwave absorbing material.

[0005] On one hand, the present invention provides a microwave absorbing material, wherein the microwave absorbing material is a hollow composite microsphere, and its structure includes:

[0006] Hollow silicate glass microspheres;

[0007] A magnetic metal layer located on the surface of the silicate glass microsphere, the magnetic metal layer being composed of several physically isolated magnetic metal regions; and

[0008] A non-magnetic metal layer is located on the magnetic metal layer, the non-magnetic metal layer being composed of a non-magnetic metal bonded to at least a portion of the magnetic metal region.

[0009] Furthermore, the non-magnetic metal is embedded in the magnetic metal in the magnetic metal region, forming a heterostructure.

[0010] Furthermore, the non-magnetic metal is embedded and connected to the magnetic metal region.

[0011] Furthermore, the magnetic metal in the magnetic metal layer will not form an alloy with the non-magnetic metal at a temperature of 600-800°C.

[0012] Furthermore, the magnetic metal layer is made of one or more magnetic metals selected from iron, cobalt, or nickel.

[0013] In this technical solution, the magnetic metal region is formed by the aggregation of magnetic metal particles. Further, the grain size of the magnetic metal is 10-100 nm, preferably 20-60 nm.

[0014] Furthermore, the non-magnetic metal is selected from copper or silver.

[0015] Furthermore, the grain size of the non-magnetic metal is 10-100 nm, preferably 20-60 nm.

[0016] Furthermore, the density of the hollow composite microspheres is 0.1-0.8 g / cm³. 3 .

[0017] Furthermore, the diameter of the hollow composite microspheres is 5-120 μm, preferably 10-70 μm.

[0018] Furthermore, in the microwave absorbing material, the total weight of the magnetic metal layer and the non-magnetic metal layer accounts for 10-70 wt% of the total weight of the microwave absorbing material, preferably 20-55 wt%. At this point, the material obtained has both good microwave absorption performance and compressive strength.

[0019] Furthermore, the weight of the magnetic metal layer accounts for 10-90 wt% of the total weight of the magnetic metal layer and the non-magnetic metal layer, preferably 30-60 wt%. At this point, the obtained material has good wave absorption performance and good compressive strength.

[0020] Furthermore, the mass ratio of the magnetic metal layer to the non-magnetic metal layer is 1:0.9-2.5, and the resulting material has both good wave absorption performance and compressive strength.

[0021] Furthermore, the total area of ​​each magnetic metal region is 20-90% of the surface area of ​​the silicate glass microspheres, preferably 50-90%, and more preferably 70-90%.

[0022] Furthermore, the average spacing between each magnetic metal region is 0.01μm-5μm, preferably 0.1-3μm, and more preferably 0.1-2μm. The material obtained under these conditions has both good wave absorption performance and compressive strength.

[0023] In another aspect, the present invention provides a method for preparing the microwave absorbing material as described above, comprising the following steps:

[0024] Hollow silicate glass microspheres were subjected to surface treatment, sensitization treatment, activation treatment and reduction treatment in sequence;

[0025] The treated silicate glass microspheres were placed in a mixed solution containing magnetic metal ions, stirred at room temperature, filtered, and dried.

[0026] The resulting substance was then placed in a mixed solution containing the aforementioned non-magnetic metal ions, stirred at room temperature, filtered, and dried.

[0027] Heat treatment yields the microwave absorbing material.

[0028] Furthermore, the hollow silicate glass microspheres undergo a flotation step before surface treatment. The flotation includes:

[0029] Hollow silicate glass microspheres were placed in a flotation solvent, mixed and stirred until homogeneous, and after standing and separating into layers, the upper floating material was taken and filtered.

[0030] Furthermore, the flotation solvent is selected from water or ethanol or a mixture of the two in any proportion.

[0031] Furthermore, the surface treatment includes: placing the hollow silicate glass microspheres in a surface treatment solution, filtering, and drying.

[0032] Furthermore, the solute in the surface treatment solution is a coupling agent.

[0033] Furthermore, the sensitization treatment includes: placing the hollow silicate glass microspheres in a sensitization solution, filtering, and drying.

[0034] Furthermore, the sensitizing solution is a reducing metal ion solution with a concentration of 0.02-0.25 mol / L.

[0035] Furthermore, the activation process includes: placing the hollow silicate glass microspheres in an activation solution, filtering, and drying.

[0036] Furthermore, the activation solution is a noble metal ion solution with a concentration of 0.002-0.2 mol / L.

[0037] Furthermore, the reduction process includes: placing the hollow silicate glass microspheres in a reducing solution, filtering, and drying.

[0038] Furthermore, the reducing solution is a solution with reducing properties and a concentration of 0.01-1.5 mol / L.

[0039] Furthermore, in the structure obtained before heat treatment, the thickness of the magnetic metal layer is 0.02-0.09 μm, and the thickness of the non-magnetic metal is 0.02-0.1 μm.

[0040] Furthermore, the heat treatment is carried out in an oxygen-free atmosphere.

[0041] Furthermore, the heat treatment is carried out under a nitrogen, argon, or hydrogen atmosphere.

[0042] Furthermore, the heat treatment temperature is 600-800℃, and the time is 1-5h.

[0043] Furthermore, the heat treatment method involves heating to 600-800℃ at a rate of 5-10℃ / min and holding at this temperature for 1-5 hours.

[0044] On another front, the present invention provides the application of the above-mentioned absorbing material in the fields of military stealth, electromagnetic radiation protection of broadcast and television transmitters, microwave anechoic chamber materials, building absorbing materials, or electromagnetic shielding materials in radio communication equipment.

[0045] Furthermore, the microwave absorbing material is used as part of a composite material in the aforementioned fields.

[0046] The beneficial effects of this invention are as follows:

[0047] The microwave absorbing material provided by this invention is a double-layered hollow metal microsphere with an island-like isolated distribution and a heterogeneous structure. It achieves low density through its internal hollow cavity and exhibits excellent compressive strength and microwave absorption properties. In the preparation method of the microwave absorbing material provided by this invention, the metal aggregation and conductivity can be controlled by adjusting different heat treatment temperatures, and its functionality can be controlled by the composition and structural design of the metal shell. Attached Figure Description

[0048] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings.

[0049] Figure 1 A schematic diagram of a microwave absorbing material structure according to the present invention is shown.

[0050] Figure 2 This diagram illustrates the process of preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure in Example 1 of the present invention.

[0051] Figure 3 The image shows a low-magnification scanning electron microscope (SEM) image of the copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure prepared in Example 1 of the present invention.

[0052] Figure 4 This image shows a high-magnification SEM image of the surface of the copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure prepared in Example 1 of the present invention.

[0053] Figure 5 This shows a high-magnification EDS image of the surface of the copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterostructure prepared in Example 1 of the present invention (and...). Figure 3 Correspondingly).

[0054] Figure 6 The image shows a high-magnification SEM image of the cross-section of the copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure prepared in Example 1 of the present invention.

[0055] Figure 7 The XRD curves of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure prepared in Example 1 of the present invention are shown.

[0056] Figure 8 The electromagnetic wave reflection loss curve of the copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure prepared in Example 1 of the present invention is shown. Detailed Implementation

[0057] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments and accompanying drawings, further explains the invention. Similar components in the drawings are indicated by the same reference numerals. Those skilled in the art should understand that the specific description below is illustrative rather than restrictive and should not be construed as limiting the scope of protection of the present invention.

[0058] This embodiment provides a wave-absorbing material, such as Figure 1 As shown, the microwave absorbing material is a hollow composite microsphere, and its structure includes:

[0059] Hollow silicate glass microspheres (glass microspheres);

[0060] A magnetic metal layer (metal 1) is located on the surface of the silicate glass microsphere, the magnetic metal layer being composed of several physically isolated magnetic metal regions; and

[0061] A non-magnetic metal layer (metal 2) is located on the magnetic metal layer (metal 1), the non-magnetic metal layer (metal 2) is composed of a non-magnetic metal, and the non-magnetic metal is bonded to at least a portion of the magnetic metal region.

[0062] Example 1

[0063] The specific implementation scheme for preparing copper-cobalt hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0064] A density of 0.39 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0065] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:2, stirred, allowed to stand and separate into layers, and the upper floating microspheres are taken and filtered.

[0066] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2, and added to silicate glass hollow microspheres at a ratio of 60g / 100mL (60g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, dried, and ready for use.

[0067] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in 0.2 mol / L stannous chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0068] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0069] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0070] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 1 g / 50 mL in a mixed solution of metal ions containing 20 g / L cobalt sulfate, 25 g / L sodium hypophosphite, 45 g / L potassium sodium tartrate, 30 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0071] Step 7: Preparation of hollow microspheres with silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 50 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0072] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 700℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the resulting bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.58 g / cm³. 3 The schematic flowchart is shown in Figure 2.

[0073] The SEM image of the hollow composite microspheres in this embodiment is shown below. Figure 3 As shown in Figures 4 and 6, the surface high-magnification EDS plots are as follows: Figure 5 As shown, the obtained hollow composite microspheres exhibit a complete spherical structure with a rough surface and aggregated particles of varying sizes. EDS spectroscopy indicates that the large particles are copper and the small particles are cobalt, with the copper and cobalt interlocking to form a heterogeneous structure. The cross-sectional SEM image clearly shows a double-layered shell composed of both silicate and metallic materials. Figure 7 The XRD curve of the bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure obtained in step 8 shows obvious diffraction peaks of copper and cobalt, indicating that even after heat treatment, no alloy was formed. Figure 8 The electromagnetic wave reflection loss curve of the bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure in this embodiment shows that the obtained hollow composite microspheres can be used as electromagnetic parameter modifiers to achieve effective absorption of electromagnetic waves; and the absorption frequency band and peak frequency can be adjusted.

[0074] Example 2

[0075] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0076] A density of 0.39 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0077] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:2, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0078] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 10:10:2. The mixture is then added to the silicate glass hollow microspheres at a ratio of 30g / 100mL (30g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, and dried for later use.

[0079] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in a 0.2 mol / L stannous chloride solution at a ratio of 1 g / 5 mL, stirred at room temperature, and filtered.

[0080] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 1 g / 5 mL, stirred at room temperature, and filtered.

[0081] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 1g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0082] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 1 g / 50 mL in a mixed solution of metal ions containing 20 g / L cobalt sulfate, 25 g / L sodium hypophosphite, 45 g / L potassium sodium tartrate, 30 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0083] Step 7: Preparation of hollow microspheres with silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 50 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0084] Step 8: Preparation of bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing nitrogen atmosphere, heated to 650℃ at a rate of 10℃ / min, and held at that temperature for 2 hours, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.58 g / cm³. 3 .

[0085] Example 3

[0086] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0087] A density of 0.31 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0088] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:1.5, stirred, allowed to stand and separate into layers, the upper floating material is taken, filtered, dried and ready for use.

[0089] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2. The mixture is then added to the silicate glass hollow microspheres at a ratio of 30g / 100mL (60g of microspheres per 100mL of solution). The mixture is stirred in a water bath for 30min, filtered, and dried for later use.

[0090] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in a 0.2 mol / L stannous chloride solution at a ratio of 1 g / 5 mL, stirred at room temperature, and filtered.

[0091] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.015 mol / L palladium chloride solution at a ratio of 1 g / 5 mL, stirred at room temperature, and filtered.

[0092] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.40 mol / L sodium hypophosphite solution at a ratio of 1 g / 5 mL, stirred at room temperature, filtered, dried and ready for use.

[0093] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 2g / 50mL in a mixed solution of metal ions containing 20g / L cobalt sulfate, 25g / L sodium hypophosphite, 45g / L potassium sodium tartrate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60℃ for 10min and then filtered.

[0094] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 50 mL of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, and 15 g / L sodium hydroxide. The mixture is stirred at room temperature for 10 min, filtered, dried, and ready for use.

[0095] Step 8: Preparation of bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 700℃ at a rate of 2℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the resulting bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.38 g / cm³. 3 .

[0096] Example 4

[0097] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0098] A density of 0.39 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0099] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:1, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0100] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:4. The mixture is then added to the silicate glass hollow microspheres at a ratio of 60g / 100mL (60g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, and dried for later use.

[0101] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in 0.2 mol / L stannous chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0102] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0103] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0104] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shells: The microspheres obtained in step 5 were treated at 1 g / 100 mL in a mixed solution of metal ions containing 20 g / L cobalt sulfate, 25 g / L sodium hypophosphite, 45 g / L potassium sodium tartrate, 30 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0105] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 50 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0106] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing nitrogen atmosphere, heated to 720℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres was 0.67 g / cm³. 3 .

[0107] Example 5

[0108] The specific implementation scheme for preparing iron-copper bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0109] A density of 0.39 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0110] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:2, stirred, allowed to stand and separate into layers, the upper floating material is taken, filtered, dried and ready for use.

[0111] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2. The mixture is then added to the silicate glass hollow microspheres at a ratio of 60g / 100mL (60g of microspheres per 100mL of solution). The mixture is stirred in a water bath for 30 minutes, filtered, and dried for later use.

[0112] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in 0.2 mol / L stannous chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0113] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0114] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0115] Step 6: Preparation of hollow microspheres with silicate-iron metal double shells: The microspheres obtained in step 5 were treated at 2g / 50ml in a mixed solution containing metal ions, namely 27g / L ferrous sulfate, 75g / L sodium potassium tartrate tetrahydrate, 2.7g / L potassium borohydride, 3g / L sucrose, and 33g / L sodium hydroxide. The mixture was stirred at room temperature for 20min and then filtered.

[0116] Step 7: Preparation of hollow microspheres with a silicate-iron-copper metal three-layer shell: The microspheres obtained in step 6 are treated in 50 mL of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, and 15 g / L sodium hydroxide. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0117] Step 8: Preparation of copper-silver bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 650℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the obtained copper-silver bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.49 g / cm³. 3 .

[0118] Example 6

[0119] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0120] A density of 0.39 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0121] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:2, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0122] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2, and added to silicate glass hollow microspheres at a ratio of 60g / 100mL (60g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, dried, and ready for use.

[0123] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in 0.2 mol / L stannous chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0124] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0125] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0126] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 1g / 50mL in a mixed solution of metal ions containing 10g / L cobalt chloride, 20g / L sodium hypophosphite, 30g / L potassium sodium tartrate, 30g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60℃ for 20min and then filtered.

[0127] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: 50 mL of the microspheres obtained in step 6 were added to a mixed solution of metal ions containing 10 g / L copper chloride, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 mL / L formaldehyde. The mixture was stirred at room temperature for 20 min, filtered, dried, and set aside for later use.

[0128] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 700℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.57 g / cm³. 3 .

[0129] Example 7

[0130] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0131] A density of 0.39 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0132] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:2, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0133] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 10:10:2. The mixture is then added to the silicate glass hollow microspheres at a ratio of 30g / 100mL (30g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, and dried for later use.

[0134] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in a 0.2 mol / L stannous chloride solution at a ratio of 1 g / 5 mL, stirred at room temperature, and filtered.

[0135] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 1 g / 5 mL, stirred at room temperature, and filtered.

[0136] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 1g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0137] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 1 g / 50 mL in a mixed solution of metal ions containing 20 g / L cobalt sulfate, 25 g / L sodium hypophosphite, 45 g / L potassium sodium tartrate, 30 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0138] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 50 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0139] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 500℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres was 0.58 g / cm³. 3 .

[0140] Example 8

[0141] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0142] A density of 0.47 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0143] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:3, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0144] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2. The mixture is then added to the silicate glass hollow microspheres at a ratio of 50g / 100mL (50g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 60℃ for 40min, filtered, and dried for later use.

[0145] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in a 0.2 mol / L stannous chloride solution at a ratio of 3 g / 5 mL, stirred at room temperature, and filtered.

[0146] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 3 g / 5 mL, stirred at room temperature, and filtered.

[0147] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0148] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 1 g / 50 mL in a mixed solution of metal ions containing 20 g / L cobalt sulfate, 25 g / L sodium hypophosphite, 45 g / L potassium sodium tartrate, 30 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0149] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 100 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0150] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 750℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.81 g / cm³. 3 .

[0151] Example 9

[0152] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0153] A density of 0.47 g / cm³ was used. 3 Commercial silicate glass hollow microspheres.

[0154] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:3, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0155] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2. The mixture is then added to the silicate glass hollow microspheres at a ratio of 50g / 100mL (50g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, and dried for later use.

[0156] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in a 0.2 mol / L stannous chloride solution at a ratio of 3 g / 5 mL, stirred at room temperature, and filtered.

[0157] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0158] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.34mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0159] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shell: The microspheres obtained in step 5 were treated at 1 g / 50 mL in a mixed solution of metal ions containing 20 g / L cobalt sulfate, 25 g / L sodium hypophosphite, 50 g / L potassium sodium tartrate, 30 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0160] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 100 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0161] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 800℃ at a rate of 5℃ / min, and held at that temperature for 3 hours, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.82 g / cm³. 3 .

[0162] Example 10

[0163] The specific implementation scheme for preparing copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure is as follows:

[0164] A density of 0.39 g / cm³ was used. 3Commercial silicate glass hollow microspheres.

[0165] The first step, flotation of silicate glass hollow microspheres: Silicate glass hollow microspheres are mixed with water at a volume ratio of 1:2, stirred, allowed to stand and separate into layers, and the upper floating material is taken and filtered.

[0166] The second step is the surface treatment of silicate glass hollow microspheres: anhydrous ethanol, distilled water, and 3-aminopropyltriethoxysilane are mixed evenly in a volume ratio of 20:10:2, and added to silicate glass hollow microspheres at a ratio of 60g / 100mL (60g of microspheres per 100mL of solution). The mixture is stirred in a water bath at 50℃ for 30min, filtered, dried, and ready for use.

[0167] The third step is the sensitization treatment of silicate glass hollow microspheres: the microspheres obtained in the second step are treated in 0.1 mol / L stannous chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0168] Step 4, activation treatment of silicate glass hollow microspheres: The microspheres obtained in step 3 are treated in 0.01 mol / L palladium chloride solution at a ratio of 2 g / 5 mL, stirred at room temperature, and filtered.

[0169] Step 5, reduction treatment of silicate glass hollow microspheres: The microspheres obtained in step 4 are treated in 0.44mol / L sodium hypophosphite solution at a ratio of 2g / 5mL, stirred at room temperature, filtered, dried and ready for use.

[0170] Step 6: Preparation of hollow microspheres with silicate-cobalt metal double shells: The microspheres obtained in step 5 were treated at 1 g / 25 mL in a mixed solution of metal ions containing 40 g / L cobalt sulfate, 50 g / L sodium hypophosphite, 100 g / L potassium sodium tartrate, 60 g / L ammonium sulfate, and pH≈10 (adjusted with ammonia). The mixture was stirred in a water bath at 60 °C for 20 min and then filtered.

[0171] Step 7: Preparation of hollow microspheres with a silicate-copper-cobalt metal three-layer shell: The microspheres obtained in step 6 are treated in 50 ml of a mixed solution of metal ions containing 20 g / L copper sulfate, 100 g / L sodium potassium tartrate, 15 g / L sodium hydroxide, and 20 ml / L formaldehyde. The mixture is stirred at room temperature for 20 min, filtered, dried, and ready for use.

[0172] Step 8: Preparation of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure: The microspheres obtained in Step 7 were placed in a flowing hydrogen atmosphere, heated to 700℃ at a rate of 5℃ / min, and held at that temperature for 1 hour, then naturally cooled to room temperature. The density of the obtained copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure was 0.58 g / cm³. 3 .

[0173] Performance testing:

[0174] Density and strength tests of copper-cobalt bimetallic hollow microspheres with island-like isolated distribution and heterogeneous structure:

[0175] Density was tested using Archimedes' principle. Strength was evaluated using isostatic pressing, referring to the patent "A method for determining the isostatic pressing strength of hollow glass microspheres" (201410196976.0), with a loading pressure of 30 MPa and a constant pressure time of 5 min.

[0176] Electromagnetic property testing of hollow composite microspheres and lightweight functional composite materials using them as fillers:

[0177] (1) Electromagnetic performance test of hollow composite microspheres: Hollow composite microspheres and paraffin were mixed at a volume ratio of 42% to prepare coaxial rings with an inner diameter of 3 mm, an outer diameter of 7 mm, and a thickness of 2 mm. The electromagnetic parameters were then tested using a vector network analyzer to analyze the electromagnetic performance. The effective absorption bandwidth is the frequency range with a reflection loss ≤ -10 dB.

[0178] (2) Electromagnetic performance test of composite material with hollow composite microspheres as filler: The prepared composite material was processed into a coaxial ring with an inner diameter of 3 mm, an outer diameter of 7 mm, and a thickness of 2 mm. The electromagnetic parameters were then tested using the coaxial method through a vector network analyzer to analyze its electromagnetic performance.

[0179] (3) The saturation magnetization intensity was measured using a vibrating sample magnetometer.

[0180] The test results are shown in Table 1 below.

[0181] In Table 1 below, the average particle spacing refers to the average spacing between each magnetic metal region.

[0182] As shown in Table 1 below, in Example 4, the excessive amount of magnetic metal used during the preparation process resulted in the absence of island-like structures in the calcined structure. Consequently, the material exhibited a low strongest reflection loss coefficient and a maximum effective absorption bandwidth of 0, indicating relatively poor absorption performance. In Example 7, due to the excessively low calcination temperature, the resulting structure also lacked island-like structures, resulting in a low strongest reflection loss coefficient and a maximum effective absorption bandwidth of 0, indicating relatively poor absorption performance.

[0183] Table 1

[0184]

[0185]

[0186] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is impossible to exhaustively list all the implementation methods here. All obvious variations or modifications derived from the technical solutions of the present invention are still within the protection scope of the present invention.

Claims

1. A microwave absorbing material, characterized in that, The microwave absorbing material is a hollow composite microsphere, the structure of which includes: Hollow silicate glass microspheres; A magnetic metal layer is located on the surface of the silicate glass microsphere, and the magnetic metal layer is composed of several magnetic metal regions that are physically isolated from each other; as well as A non-magnetic metal layer is located on the magnetic metal layer, the non-magnetic metal layer being composed of a non-magnetic metal, the non-magnetic metal being bonded to at least a portion of the magnetic metal region.

2. The microwave absorbing material according to claim 1, characterized in that, The magnetic metal in the magnetic metal layer will not form an alloy with the non-magnetic metal at a temperature of 600-800℃.

3. The microwave absorbing material according to claim 2, characterized in that, The magnetic metal layer is made of one or more magnetic metals selected from iron, cobalt, or nickel. The grain size of the magnetic metal is 10-100 nm.

4. The microwave absorbing material according to claim 3, characterized in that, The grain size of the magnetic metal is 20-60 nm.

5. The microwave absorbing material according to claim 2, characterized in that, The non-magnetic metal is selected from copper or silver; The grain size of the non-magnetic metal is 10-100 nm.

6. The microwave absorbing material according to claim 5, characterized in that, The grain size of the non-magnetic metal is 20-60 nm.

7. The microwave absorbing material according to claim 1, characterized in that, The density of the hollow composite microspheres is 0.1-0.8 g / cm³. 3 The diameter of the hollow composite microspheres is 5-120 μm.

8. The microwave absorbing material according to claim 7, characterized in that, The diameter of the hollow composite microspheres is 10-70 μm.

9. The microwave absorbing material according to claim 1, characterized in that, In the aforementioned microwave absorbing material, the total weight of the magnetic metal layer and the non-magnetic metal layer accounts for 10-70 wt% of the total weight of the microwave absorbing material. The weight of the magnetic metal layer accounts for 10-90 wt% of the total weight of the magnetic metal layer and the non-magnetic metal layer.

10. The microwave absorbing material according to claim 9, characterized in that, In the microwave absorbing material, the total weight of the magnetic metal layer and the non-magnetic metal layer accounts for 20-55 wt% of the total weight of the microwave absorbing material.

11. The microwave absorbing material according to claim 10, characterized in that, The magnetic metal layer accounts for 30-60 wt% of the total weight of the magnetic metal layer and the non-magnetic metal layer.

12. The microwave absorbing material according to claim 1, characterized in that, The total area of ​​each magnetic metal region is 20-90% of the surface area of ​​the silicate glass microspheres; The average spacing between each magnetic metal region is 0.01μm-5μm.

13. The microwave absorbing material according to claim 12, characterized in that, The total area of ​​each magnetic metal region is 50-90% of the surface area of ​​the silicate glass microspheres.

14. The microwave absorbing material according to claim 13, characterized in that, The total area of ​​each magnetic metal region is 70-90% of the surface area of ​​the silicate glass microspheres.

15. The microwave absorbing material according to claim 1, characterized in that, The average spacing between each magnetic metal region is 0.1-3 μm.

16. The method for preparing the microwave absorbing material according to any one of claims 1-15, characterized in that, Includes the following steps: Hollow silicate glass microspheres were subjected to surface treatment, sensitization treatment, activation treatment and reduction treatment in sequence; The treated silicate glass microspheres were placed in a mixed solution containing magnetic metal ions, stirred at room temperature, filtered, and dried. The resulting substance was then placed in a mixed solution containing the aforementioned non-magnetic metal ions, stirred at room temperature, filtered, and dried. Heat treatment yields the microwave absorbing material.

17. The preparation method according to claim 16, characterized in that, Before heat treatment, the resulting structure has a magnetic metal layer thickness of 0.02-0.09 μm and a non-magnetic metal layer thickness of 0.02-0.1 μm.

18. The preparation method according to claim 16, characterized in that, The heat treatment is carried out in an oxygen-free atmosphere.

19. The preparation method according to claim 18, characterized in that, The heat treatment is carried out in a nitrogen, argon, or hydrogen atmosphere.

20. The preparation method according to claim 16, characterized in that, The heat treatment is performed at a temperature of 600-800℃ for 1-5 hours.

21. The application of the microwave absorbing material as described in any one of claims 1-15 in the fields of military stealth, electromagnetic radiation protection of radio and television transmitters, microwave anechoic chamber materials, building microwave absorbing materials, or electromagnetic shielding materials in radio communication equipment.

Citation Information

Patent Citations

  • Method for measuring isostatic pressure resistance of hollow glass beads

    CN103954506A

  • High-temperature-resistant radar and infrared compatible stealth coating and preparation method thereof

    CN108212722A

  • Carbon-magnetic metal dispersion type hollow composite microsphere as well as preparation method and application thereof

    CN114073919A