A method and device for preparing ternary precursor material for sodium ion battery
By controlling the precipitation and growth process of the ternary precursor material of sodium ion battery under an inert gas atmosphere, the problem of material density and activity is solved, and the circulation ability and stability of the positive electrode material of sodium ion battery are improved.
Patent Information
- Application Number
- CN202311513150.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-11-10
AI Technical Summary
The tap density and activity of the ternary precursor material of sodium ion battery are low and have too high activity, resulting in cracks in the structure of the sintered positive electrode material, affecting the circulation ability.
The precipitant, complexing agent and chelating agent are added to pure water or deionized water under an inert gas atmosphere and stirred to control the pH and ammonia water concentration, and the flow rate and pH are adjusted through the co-precipitation reaction and passivation stage to reduce the stirring speed and pH. Prevent the surface activity of the crystal nucleus from being too strong and agglomerated, gradually reduce the activity of the material surface, and ensure stable crystal growth.
The obtained sodium ion battery ternary precursor material has a high tap density (1.8-2.2g/cm3), good spherical shape, and is not easily oxidized by air, which improves the circulation ability and long circulation performance of the sodium ion battery positive electrode material.
Smart Images

Figure CN117800404B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing a ternary precursor material for a sodium ion battery and a device for preparing a ternary precursor material for a sodium ion battery based on the method. Background Art
[0002] Sodium-ion battery is a secondary battery (rechargeable battery) that mainly relies on the movement of sodium ions between the positive electrode and the negative electrode to work, similar to the working principle of lithium-ion battery. Since the positive electrode material of ternary sodium-ion battery has a layered oxide structure similar to that of ternary lithium-ion battery positive electrode material, and multiple metal elements play different roles in the material structure, the stability and specific capacity of the positive electrode material of sodium-ion battery are relatively high, but its long-cycle performance has certain limitations. It is necessary to optimize the structure of the positive electrode material of ternary sodium-ion battery to improve the long-cycle performance of sodium-ion battery.
[0003] At present, the main means of optimizing the long-cycle performance of sodium-ion batteries is to dope or coat the positive electrode materials to further improve the performance of the positive electrode materials. Since the positive electrode materials of sodium-ion batteries are made by sintering hydroxide precursors and sodium salts, the cycle capacity of the positive electrode materials of sodium-ion batteries can also be improved by optimizing the precursors, thereby improving the long-cycle performance of sodium-ion batteries. At present, the tap density of the ternary precursor materials of sodium-ion batteries is low, and there are problems such as excessive activity and easy deterioration, which leads to cracks in the structure of the sintered positive electrode materials and has an adverse effect on the cycle capacity of the positive electrode materials of sodium-ion batteries. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a ternary precursor material for a sodium ion battery and a device for preparing a ternary precursor material for a sodium ion battery based on the method for preparing a ternary precursor material for a sodium ion battery, which solves the problems of low tap density and excessive activity of the ternary precursor material for a sodium ion battery in the prior art.
[0005] According to an embodiment of the present invention, a method for preparing a ternary precursor material for a sodium ion battery comprises the following steps:
[0006] S1, solution preparation stage: use divalent nickel salt solution, divalent iron salt solution and divalent manganese salt solution to prepare a mixed metal salt solution. 2+ , Fe 2+ , Mn 2+The total molar concentration is 1.50-2.50 mol / L; 6.00-12.00 mol / L sodium hydroxide solution is prepared as a precipitant; 5.00-10.00 mol / L ammonia solution is prepared as a complexing agent; 0.01-0.05 mol / L sodium gluconate solution is prepared as a chelating agent;
[0007] S2, base liquid preparation stage: in an inert gas atmosphere, add a precipitant, a complexing agent and a chelating agent to pure water or deionized water and stir to obtain a base liquid, the stirring speed is 50.00-100.00 rpm, and the temperature is raised to 50.00-60.00° C. while stirring, the concentration of ammonia water in the base liquid is 3.00-8.00 g / L and the pH of the base liquid is adjusted to 12.00-13.00;
[0008] S3, nucleation stage: in an inert gas atmosphere, continuously add a mixed metal salt solution, a precipitant, a complexing agent and a chelating agent to the base liquid and stir to perform a co-precipitation reaction, increase the stirring speed to more than 350.00 rpm, and control the pH to be maintained at 12.00-12.30, and the concentration of ammonia water to be maintained at 5.00-8.00 g / L, for 1.00-10.00 h;
[0009] S4, passivation stage: under an inert gas atmosphere, control the pH to drop to 11.60-11.90, and increase the flow rate of the mixed metal salt solution to 1.50-3.00 times the original flow rate, continue to add the mixed metal salt solution, precipitant, complexing agent and chelating agent and stir, and control the concentration of ammonia water to drop to 3.00-7.00 g / L, and continue for 6.00-20.00 hours;
[0010] S5, growth stage: under an inert gas atmosphere, control the pH to drop to 11.00-11.60, increase the flow rate of the mixed metal salt solution to 1.50-3.00 times of the original flow rate, continue to add the mixed metal salt solution, precipitant, complexing agent and chelating agent and stir, and the stirring speed is reduced to 200.00-300.00rpm, and the ammonia concentration is reduced to 3.00-6.00g / L, and stop discharging after 30.00-180.00h to obtain slurry;
[0011] S6, post-processing stage: ageing, washing, drying and screening the slurry to obtain the sodium ion battery ternary precursor material.
[0012] On the other hand, according to an embodiment of the present invention, a sodium ion battery ternary precursor material preparation device is also provided, which is used to implement the above-mentioned sodium ion battery ternary precursor material preparation method, including a reactor, a first container, a second container, a third container, a fourth container, a water tank and an inert gas tank, the first container, the second container, the third container, the fourth container, the water tank and the inert gas tank are respectively connected to the reactor, the first container stores a mixed metal salt solution, the second container stores a precipitant, the third container stores a complexing agent, the fourth container stores a chelating agent, the water tank stores pure water or deionized water, and the inert gas tank stores an inert gas.
[0013] Compared with the prior art, the present invention has the following beneficial effects: by adding a precipitant, a complexing agent and a chelating agent to pure water or deionized water under an inert gas atmosphere and stirring to obtain a base liquid, the mixed metal salt solution is injected into the base liquid more slowly in the nucleation stage than in the later passivation stage and the growth stage, so as to prevent the excessive surface activity of the crystal nucleus in the initial nucleation stage from causing the material to agglomerate and affect the sphericity of the later crystallization, and in the passivation stage, the pH is lowered and the flow rate of the mixed metal salt solution injected is increased, so as to increase the solid content of the reaction liquid, and the activity of the surface of the material is gradually reduced and tends to be stable during the reaction process. , effectively avoiding secondary nucleation or agglomeration of the material, and finally increasing the injection flow of the mixed metal salt solution and reducing the stirring speed and pH. In this stage, the crystal grows stably, and the material slurry generated in the growth stage is post-treated to obtain the sodium ion battery ternary precursor material, that is, by controlling the injection flow of the mixed metal salt solution, precipitant, complexing agent and chelating agent in the nucleation stage, passivation stage and growth stage, the pH and ammonia concentration of the reaction solution are accurately controlled to prevent agglomeration during the coprecipitation reaction, and the sodium gluconate in the chelating agent is used to chelate the Fe 2+ Fe produced by oxidation 3+ Coordinate, greatly weakening Fe 3+ With OH - reaction, reducing Fe 3+ With OH - The reaction produces loose iron hydroxide precipitation to avoid Fe 3+ Participate in the coprecipitation reaction, which solves the technical problems of low tap density and high activity of the existing sodium ion battery ternary precursor materials, and produces a tap density of 1.8-2.2g / cm 3 The technical effect of high tap density sodium ion battery ternary precursor material is achieved, and the prepared sodium ion battery ternary precursor material has good sphericity and is not easily oxidized by air, which improves the cycle capacity of the sodium ion battery positive electrode material prepared by sintering the sodium ion battery ternary precursor material with sodium salt, thereby improving the long cycle capacity of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a schematic structural diagram of a device for preparing a ternary precursor material for a sodium ion battery according to Embodiment 1 of the present invention;
[0015] Figure 2 It is a cross-sectional view of a reaction kettle in a sodium ion battery ternary precursor material preparation device according to Example 1 of the present invention;
[0016] Figure 3 This is a SEM image of a sodium ion battery ternary precursor material prepared by the method for preparing a sodium ion battery ternary precursor material according to Example 2 of the present invention;
[0017] Figure 4 This is a cross-sectional view of a sodium ion battery ternary precursor material prepared by the method for preparing a sodium ion battery ternary precursor material according to Example 2 of the present invention;
[0018] Figure 5 This is a SEM image of a sodium ion battery ternary precursor material prepared by the method for preparing a sodium ion battery ternary precursor material according to Example 3 of the present invention;
[0019] Figure 6 This is a cross-sectional view of a sodium ion battery ternary precursor material prepared by the method for preparing a sodium ion battery ternary precursor material according to Example 3 of the present invention;
[0020] Figure 7 This is a SEM image of a sodium ion battery ternary precursor material prepared by the method for preparing a sodium ion battery ternary precursor material according to Example 4 of the present invention;
[0021] Figure 8 This is a cross-sectional view of a sodium ion battery ternary precursor material prepared by the method for preparing a sodium ion battery ternary precursor material according to Example 4 of the present invention.
[0022] In the above drawings: 1. Reactor; 2. First container; 3. Second container; 4. Third container; 5. Fourth container; 6. Water tank; 7. Inert gas tank; 8. Pipeline; 9. Valve; 10. Mortar pump; 11. Temporary storage tank; 12. Concentrator; 13. Reflux pipe; 14. Reflux valve; 15. Stirring shaft; 16. First stirring blade; 17. Stirring plate; 18. Second stirring blade; 19. Third stirring blade; 20. Baffle. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0024] Embodiment 1
[0025] like Figure 1 and Figure 2As shown, the first embodiment of the present invention provides a sodium ion battery ternary precursor material preparation device, which is used to prepare a sodium ion battery ternary precursor material. The chemical formula of the sodium ion battery ternary precursor material is Ni x Fe y Mn z (OH) 2 , wherein x=0.20-0.40, y=0.20-0.40, y=0.20-0.40 and x+y+z=1, and the obtained nickel-iron-manganese hydroxide has a specific surface area of 3.00-8.50 m2 / g and a tap density of 1.70-2.60 g / cm 3 , bulk density is 1.00-1.50g / cm 3 , D50 is 2.00-8.00 μm, particle size distribution (D90-D10) / D50 is 0.65-0.90, sodium content is less than 200.00 ppm, sulfur content is less than 1500.00 ppm, and the nickel-iron-manganese hydroxide has good overall sphericity, all of which are regular spheres, the primary particles are short and thick blocks and are extremely densely distributed, with good crystallinity and not easily oxidized by air.
[0026] Please refer to Figure 1 The sodium ion battery ternary precursor material preparation device includes a reactor 1, a first container 2, a second container 3, a third container 4, a fourth container 5, a water tank 6 and an inert gas tank 7, wherein the first container 2, the second container 3, the third container 4, the fourth container 5, the water tank 6 and the inert gas tank 7 are respectively connected to the reactor 1 through a pipeline 8, and the pipeline 8 is respectively provided with a valve 9 for controlling the on-off of the pipeline 8, the first container 2 stores a mixed metal salt solution, the second container 3 stores a precipitant, the third container 4 stores a complexing agent, the fourth container 5 stores a chelating agent, the water tank 6 stores pure water or deionized water, and the inert gas Inert gas is stored in the tank 7. By controlling the opening and closing of the corresponding pipeline 8 through the valve 9, the mixed metal salt solution stored in the first container 2, the precipitant stored in the second container 3, the complexing agent stored in the third container 4, the chelating agent stored in the fourth container 5, the pure water or deionized water stored in the water tank 6, and the inert gas stored in the inert gas tank 7 can be input into the reactor 1 for reaction, and the flow rates of the mixed metal salt solution, the precipitant, the complexing agent, the chelating agent, the pure water or deionized water and the inert gas input into the reactor 1 can be changed respectively by adjusting the opening of each of the regulating valves 9. The inert gas stored in the inert gas pipe can be nitrogen, helium, etc.
[0027] like Figure 1As shown, the sodium ion battery ternary precursor material preparation device also includes a mortar pump 10, a temporary storage tank 11, a concentrator 12 and a reflux pipe 13. The reactor 1, the mortar pump 10, the temporary storage tank 11 and the concentrator 12 are connected in sequence. The reflux pipe 13 connects the concentrator 12 and the reactor 1 to form a loop, and the reflux pipe 13 is provided with a reflux valve 14 for controlling the on-off of the reflux pipe 13.
[0028] Specifically, after the reaction liquid in the reactor 1 is full, the reaction liquid in the reactor 1 is pumped into the temporary storage tank 11 by the mortar pump 10, and flows into the concentrator 12 from the temporary storage tank 11. The concentrator 12 performs pressure filtration on the reaction liquid and then discharges the filtrate. The concentrated liquid after pressure filtration by the concentrator 12 is refluxed into the reactor 1 through the reflux pipe 13 to increase the solid content of the reaction liquid in the reactor 1. By controlling the flow rate of the mortar pump 10 and the opening of the reflux valve 14, the liquid level in the reactor 1, the liquid level in the temporary storage tank 11 and the liquid level in the concentrator 12 can be kept constant, thereby avoiding overflow.
[0029] Optionally, the volume of the reactor 1 is 4.00-10.00m 3 The volume of the concentrator 12 is 0.50-3.00m 3 The volume of the reactor 1 and the volume of the concentrator 12 are selected according to actual production requirements.
[0030] like Figure 2 As shown, a rotatable stirring shaft 15 is provided in the reactor 1, and a first stirring assembly, a second stirring assembly and a third stirring assembly are provided on the stirring shaft 15 at intervals in the vertical direction. The first stirring assembly includes a plurality of first stirring blades 16, and the angle between the first stirring blades 16 and the horizontal plane is 30.00-60.00°. The second stirring assembly includes a stirring plate 17 and a plurality of second stirring blades 18 arranged on the stirring plate 17, and the angle between the second stirring blades 18 and the horizontal plane is 45.00°. The third stirring assembly includes a plurality of third stirring blades 19, and the angle between the third stirring blades 19 and the horizontal plane is 30.00-60.00°. The inclination direction of the third stirring blades 19 is opposite to the inclination direction of the first stirring blades 16. The rotation of the stirring shaft 15 drives the first stirring assembly, the second stirring assembly and the third stirring assembly to rotate synchronously, so that the reaction liquid in the reactor 1 can be fully stirred to ensure that the components in the reaction liquid fully interact with each other.
[0031] In detail, a plurality of baffles 20 are further provided on the inner wall of the reactor 1, and the baffles 20 extend in a direction close to the stirring shaft 15 and are arranged at intervals along the circumference of the stirring shaft 15. By providing the baffles 20 to block the reaction liquid from flowing in the reactor 1, when the first stirring component, the second stirring component, the third stirring component and the baffles 20 are used in combination, the mixing degree of the reaction liquid in the reactor 1 can be further improved, which is conducive to the smooth progress of the reaction.
[0032] Please refer to Figure 2 In the reactor 1, the connection point between the pipeline 8 connected with the first container 2 and the reactor 1, the connection point between the pipeline 8 connected with the second container 3 and the reactor 1, the connection point between the pipeline 8 connected with the third container 4 and the reactor 1, and the connection point between the pipeline 8 connected with the fourth container 5 and the reactor 1 are all located on the side of the second stirring component, so that after the mixed metal salt solution, precipitant, complexing agent and chelating agent are injected into the reactor 1, they can flow and mix rapidly in the reactor 1 driven by the second stirring component.
[0033] Specifically, two groups of second stirring blades 18 are provided on the stirring disk 17 of the second stirring component, wherein one group of the second stirring blades 18 is close to the edge of the stirring disk 17 and the second stirring blades 18 of this group are in a straight line, so that the second stirring component can generate a strong shear force during the rotation process, and the other group of the second stirring blades 18 is close to the stirring shaft 15 and the second stirring blades 18 of this group are in a right angle, which is used to prevent part of the reaction liquid from being retained above and below the stirring disk 17 during the rotation of the second stirring component, and to prevent the particles in the reaction liquid from agglomerating due to dead corners in the reactor 1, and the second stirring blades 18 close to the stirring shaft 15 during the rotation of the second stirring component can push The reaction liquid is driven to flow toward the direction close to the first stirring component and the third stirring component respectively. At the same time, the reaction liquid is pushed close to the second stirring component during the rotation of the first stirring component and the second stirring component, so that the reaction liquid collides and is fully mixed in the reactor 1. Therefore, during the rotation of the stirring shaft 15, a strong shear force is generated on the reaction liquid in the area where the first stirring blade 16 rotates, the area where the second stirring blade 18 rotates near the edge of the stirring disk 17, the area where the third stirring blade 19 rotates, and the area where the reaction liquid collides, so that the components of the reaction liquid are fully mixed and reacted, so that the prepared sodium ion battery ternary precursor material has the properties of low activity, high tap density and high sphericity appearance.
[0034] Embodiment 2
[0035] like Figure 3 and Figure 4As shown, a method for preparing a sodium ion battery ternary precursor material is based on the sodium ion battery ternary precursor material preparation device in Example 1, and is used to prepare a sodium ion battery ternary precursor material with a particle size D50 = 2.50 μm.
[0036] The method for preparing a ternary precursor material for a sodium ion battery comprises the following steps:
[0037] S1, solution preparation stage: use divalent nickel salt solution, divalent iron salt solution and divalent manganese salt solution to prepare a mixed metal salt solution. 2+ , Fe 2+ , Mn 2+ The total molar concentration is 1.50 mol / L; 12.00 mol / L sodium hydroxide solution is prepared as a precipitant; 8.30 mol / L ammonia solution is prepared as a complexing agent; and 0.03 mol / L sodium gluconate solution is prepared as a chelating agent.
[0038] In step S1, Ni in the mixed metal salt solution 2+ , Fe 2+ , Mn 2+ The molar ratio of is 2:5:3, and the divalent nickel salt is nickel sulfate, the divalent iron salt is ferrous sulfate, and the divalent manganese salt is manganese sulfate. The above raw materials are respectively dissolved in pure water to prepare a mixed metal salt solution.
[0039] In step S1, sodium gluconate solution is selected as a chelating agent. Sodium gluconate is a polyhydroxy acid type slow-release scale inhibitor. 3+ Has good coordination ability, due to the Fe 2+ The stability is poor, some Fe 2+ Will be oxidized to Fe 3+ At the appropriate concentration ratio, sodium gluconate can react with Fe 3+ The specific coordination greatly weakens the Fe 3+ With OH - reaction, reducing Fe 3+ With OH - The reaction produces a loose precipitate of iron hydroxide, and sodium gluconate and Fe 3+ The formed chelate will be discharged during the subsequent concentrator pressure filtration of the reaction solution, effectively reducing the Fe 3+ With OH - The adverse effects of the reaction are eliminated, and sodium gluconate can modify the surface of the material particles to a certain extent and produce a polishing effect, which is beneficial to improving the quality of the finished product.
[0040] Step S2: add a volume of 6.00m 3 Add 2.00m3 of pure water and nitrogen was introduced from the bottom of the reactor, the stirring shaft was turned on and the temperature was raised to 50.00°C, the stirring speed of the stirring shaft was 100.00rpm, a precipitant, a complexing agent and a chelating agent were added in sequence, the pH of the reaction solution in the reactor was adjusted to 13.00 and the concentration of ammonia water to 6.50g / L, and a bottom liquid was obtained.
[0041] Step S3, nucleation stage: the stirring speed of the stirring shaft is increased to 380.00rpm, the nitrogen outlet for injecting nitrogen into the reactor is switched from the bottom of the reactor to the top of the reactor and the nitrogen flow rate is maintained at 40.00L / h; a mixed metal salt solution, a precipitant, a complexing agent and a chelating agent are continuously added to the bottom liquid for a co-precipitation reaction, wherein the feed flow rate of the metal salt mixed solution is 50.00L / h, the feed flow rate of the mixed metal salt molten solution, the feed flow rate of the precipitant, the feed flow rate of the complexing agent and the feed flow rate of the chelating agent are 40:15:1:2, and the temperature in the reactor is controlled to be maintained at 50.00±1.00℃, the pH is maintained at 12.30, and the concentration of ammonia water is maintained at 5.00g / L for 6.00h.
[0042] Step S4, passivation stage: the pH in the reactor is reduced to 11.90 at a rate of 0.10 per hour, and the feed flow rate of the mixed metal solution is increased to 100.00L / h, the feed flow rate of the complexing agent is adjusted according to the ratio of the feed flow rate of the complexing agent to the feed flow rate of the mixed metal salt solution in step S3, and the feed flow rate of the chelating agent is adjusted according to the ratio of the feed flow rate of the chelating agent to the feed flow rate of the mixed metal salt solution in step S3. The temperature in the reactor is controlled to be maintained at 50.00±1.00℃, the pH is maintained at 11.85-11.90, and the concentration of ammonia water is maintained at 4.00g / L for 10.00h.
[0043] In step S4, the growth of the crystal generally includes the following stages: micro-mixing of the reactants, formation of ordered crystal primitives, orderly bonding of the crystal primitives to form ordered crystal nuclei, and superposition of the crystal primitives on the crystal nuclei to make the crystal nuclei grow. Since the crystal primitives are highly active, unstable and easy to agglomerate, excessively high pH and ammonia concentrations will cause excessive agglomeration of the crystal primitives, and the particles generated by agglomeration will have low strength, and will easily crack to form multiple irregular small particles during the subsequent high-temperature sintering process, and will have an adverse effect on the electrical performance indicators of the positive electrode material. Excessively low pH and ammonia concentrations will cause the crystal primitives to bond to the crystal nuclei too quickly and the bonding will change from ordered to disordered, resulting in a wide distribution of the particle size of the formed particles and containing a large number of particles with small particle sizes, resulting in poor cycle performance of the positive electrode material obtained by high-temperature sintering. Therefore, after the reactants are slightly mixed and form crystal units in step S3, it is necessary to adjust the pH and ammonia concentration in the reactor in step S4 and maintain the pH and ammonia concentration of the reaction liquid in the reactor within an appropriate range to prevent the crystal units from agglomerating. When the crystal units in the reactor continue to decrease, the crystal nuclei formed by bonding can have a higher sphericity and the surface of the primary particles can be roughened, thereby reducing the free energy and activity of the crystal nuclei surface and inhibiting the occurrence of agglomeration.
[0044] In step S4, after the reaction liquid in the reactor is full, the mortar pump and the concentrator are turned on to filter the reaction liquid and discharge the filtrate. At the same time, the concentrated liquid is refluxed into the reactor through the reflux pipe to increase the solid content in the reactor and ensure the stability of the liquid level in the reactor and the concentrator.
[0045] Step S5, growth stage: the rotation speed of the stirring shaft is reduced to 200.00 rpm at a rate of 10.00 rpm per hour, the pH in the reactor is reduced to 11.60 at a rate of 0.10 per hour, the feed flow rate of the complexing agent is reduced to reduce the concentration of the ammonia water in the reactor to 3.00 g / L at a rate of 0.20 g / L per hour, and the feed flow rate of the mixed metal solution is increased to 300.00 L / h, the feed flow rate of the chelating agent is adjusted according to the ratio of the feed flow rate of the chelating agent to the feed flow rate of the mixed metal salt solution in step S3, the temperature in the reactor is controlled to be maintained at 50.00±1.00°C, the pH is maintained at 11.55-11.60, and the concentration of the ammonia water is maintained at 3.00 g / L, and the discharge is stopped after 30.00-80.00 hours to obtain a slurry.
[0046] In step S5, the duration of the reaction is confirmed based on the particle size D50 of the material in the slurry, and the particle size of the material is detected. When the particle size D50 of the detected material reaches 2.50μm and the reaction time of step 5 is within the range of 30.00-80.00h, the reactor can be stopped and the material can be discharged; if the reaction time has reached 30.00h and the particle size has not reached 2.50μm, the reaction is continued for a period of time until the particle size of the material meets the standard and then the reactor is stopped and the material is discharged; if the reaction time has reached 80.00h, and the particle size has not reached 2.50μm and the difference with 2.50μm is within the allowable range (10.00%), the reactor can be stopped in advance and the material can be discharged.
[0047] Step S6, post-processing stage: ageing, washing, drying and sieving the slurry to obtain a sodium ion battery ternary precursor material.
[0048] In step S6, nitrogen is first introduced into the aging tank for protection, and then the slurry in the reactor is put into the aging tank for stirring. The aging lasts for 8-10 hours, and then the aged rubber material is washed, dried, and sieved to obtain nickel iron manganese hydroxide with a particle size of D50=2.50μm. The obtained nickel iron manganese hydroxide is packaged to obtain a finished sodium ion battery ternary precursor material.
[0049] In order to prevent the chelating agent from decomposing too quickly during the reaction, step S1 also includes diluting hydrazine hydrate and water at a ratio of 1.00:100.00 to prepare a reducing solvent; step S2 also includes adding a reducing solvent to pure water or deionized water; step S3 also includes continuously adding a reducing solvent to the base liquid; step S4 also includes continuously adding a reducing solvent; step S5 also includes continuously adding a reducing solvent.
[0050] like Figure 3 and Figure 4 As shown, the inner and outer layers of the sodium ion battery ternary precursor material prepared by the method for preparing the sodium ion battery ternary precursor material provided in this embodiment are both compact in morphology, and the outer layer is in a state of large and tightly packed blocks, so that air is not easy to enter the interior of the particles, that is, the Fe inside the particles 2+ It is difficult to be oxidized by air at room temperature, which helps prevent the material from being oxidized during aging and washing.
[0051] Embodiment 3
[0052] like Figure 5 and Figure 6 As shown, a method for preparing a sodium ion battery ternary precursor material is based on the sodium ion battery ternary precursor material preparation device in Example 1, and is used to prepare a sodium ion battery ternary precursor material with a particle size D50 = 5.00 μm.
[0053] The method for preparing a ternary precursor material for a sodium ion battery comprises the following steps:
[0054] S1, solution preparation stage: use divalent nickel salt solution, divalent iron salt solution and divalent manganese salt solution to prepare a mixed metal salt solution. 2+ , Fe 2+ , Mn 2+ The total molar concentration is 2.00 mol / L; a 6.00 mol / L sodium hydroxide solution is prepared as a precipitant; a 5.00 mol / L ammonia solution is prepared as a complexing agent; and a 0.01 mol / L sodium gluconate solution is prepared as a chelating agent.
[0055] In step S1, Ni in the mixed metal salt solution 2+ , Fe 2+ , Mn 2+ The molar ratio of is 2:5:3, and the divalent nickel salt is nickel nitrate, the divalent iron salt is ferrous nitrate, and the divalent manganese salt is manganese nitrate. The above raw materials are respectively dissolved in pure water to prepare a mixed metal salt solution.
[0056] Step S2: add a volume of 6.00m 3 Add 2.00m 3 of pure water and nitrogen was introduced from the bottom of the reactor, the stirring shaft was turned on and the temperature was raised to 55.00°C, the stirring speed of the stirring shaft was 50.00 rpm, a precipitant, a complexing agent and a chelating agent were added in sequence, the pH of the reaction solution in the reactor was adjusted to 12.50 and the concentration of ammonia water to 7.00 g / L, and a bottom liquid was obtained.
[0057] Step S3, nucleation stage: the stirring speed of the stirring shaft is increased to 360.00rpm, the nitrogen outlet for injecting nitrogen into the reactor is switched from the bottom of the reactor to the top of the reactor and the nitrogen flow rate is maintained at 200.00L / h; a mixed metal salt solution, a precipitant, a complexing agent and a chelating agent are continuously added to the bottom liquid for a co-precipitation reaction, wherein the feed flow rate of the metal salt mixed solution is 50.00L / h, the feed flow rate of the mixed metal salt molten solution, the feed flow rate of the precipitant, the feed flow rate of the complexing agent and the feed flow rate of the chelating agent are 40:15:1:2, and the temperature in the reactor is controlled to be maintained at 55.00±1.00℃, the pH is maintained at 12.20, and the concentration of ammonia water is maintained at 8.00g / L for 4.00h.
[0058] Step S4, passivation stage: the pH in the reactor is reduced to 11.70 at a rate of 0.05 per hour, and the feed flow rate of the mixed metal solution is increased to 150.00 L / h, the feed flow rate of the complexing agent is adjusted according to the ratio of the feed flow rate of the complexing agent to the feed flow rate of the mixed metal salt solution in step S3, and the feed flow rate of the chelating agent is adjusted according to the ratio of the feed flow rate of the chelating agent to the feed flow rate of the mixed metal salt solution in step S3. The temperature in the reactor is controlled to be maintained at 55.00±1.00°C, the pH is maintained at 11.65-11.70, and the concentration of ammonia water is maintained at 7.00 g / L for 10.00 h.
[0059] In step S4, after the reaction liquid in the reactor is full, the mortar pump and the concentrator are turned on to filter the reaction liquid and discharge the filtrate. At the same time, the concentrated liquid is refluxed into the reactor through the reflux pipe to increase the solid content in the reactor and ensure the stability of the liquid level in the reactor and the concentrator.
[0060] Step S5, growth stage: the rotation speed of the stirring shaft is reduced to 300.00 rpm at a rate of 5.00 rpm per hour, the pH in the reactor is reduced to 11.50 at a rate of 0.15 per hour, the feed flow rate of the complexing agent is reduced to reduce the concentration of the ammonia water in the reactor to 6.00 g / L at a rate of 0.50 g / L per hour, and the feed flow rate of the mixed metal solution is increased to 450.00 L / h, the feed flow rate of the chelating agent is adjusted according to the ratio of the feed flow rate of the chelating agent to the feed flow rate of the mixed metal salt solution in step S3, the temperature in the reactor is controlled to be maintained at 55.00±1.00°C, the pH is maintained at 11.45-11.50, and the concentration of the ammonia water is maintained at 6.00 g / L, and the discharge is stopped after 50.00-100.00 hours to obtain a slurry.
[0061] In step S5, the duration of the reaction is confirmed based on the particle size D50 of the material in the slurry, and the particle size of the material is detected. When the particle size D50 of the detected material reaches 5.00μm and the reaction time of step 5 is within the range of 50.00-100.00h, the reactor can be stopped and the material can be discharged; if the reaction time has reached 50.00h and the particle size has not reached 5.00μm, the reaction is continued for a period of time until the particle size of the material meets the standard and then the reactor is stopped and the material is discharged; if the reaction time has reached 100.00h, and the particle size has not reached 5.00μm and the difference with 5.00μm is within the allowable range (10.00%), the reactor can be stopped in advance and the material can be discharged.
[0062] Step S6, post-processing stage: ageing, washing, drying and sieving the slurry to obtain a sodium ion battery ternary precursor material.
[0063] In step S6, nitrogen is first introduced into the aging tank for protection, and then the slurry in the reactor is put into the aging tank for stirring. The aging lasts for 8-10 hours, and then the aged rubber material is washed, dried, and sieved to obtain nickel iron manganese hydroxide with a particle size of D50=5.00μm. The obtained nickel iron manganese hydroxide is packaged to obtain a finished sodium ion battery ternary precursor material.
[0064] In order to prevent the chelating agent from decomposing too quickly during the reaction, step S1 also includes diluting hydrazine hydrate and water at a ratio of 1.00:100.00 to prepare a reducing solvent; step S2 also includes adding a reducing solvent to pure water or deionized water; step S3 also includes continuously adding a reducing solvent to the base liquid; step S4 also includes continuously adding a reducing solvent; step S5 also includes continuously adding a reducing solvent.
[0065] Embodiment 4
[0066] like Figure 7 and Figure 8 As shown, a method for preparing a sodium ion battery ternary precursor material is based on the sodium ion battery ternary precursor material preparation device in Example 1, and is used to prepare a sodium ion battery ternary precursor material with a particle size of D50=7.50μm.
[0067] The method for preparing a ternary precursor material for a sodium ion battery comprises the following steps:
[0068] S1, solution preparation stage: use divalent nickel salt solution, divalent iron salt solution and divalent manganese salt solution to prepare a mixed metal salt solution. 2+ , Fe 2+ , Mn 2+ The total molar concentration is 2.50 mol / L; 10.80 mol / L sodium hydroxide solution is prepared as a precipitant; 10.00 mol / L ammonia solution is prepared as a complexing agent; and 0.05 mol / L sodium gluconate solution is prepared as a chelating agent.
[0069] In step S1, Ni in the mixed metal salt solution 2+ , Fe 2+ , Mn 2+ The molar ratio of is 2:5:3, and the divalent nickel salt is nickel chloride, the divalent iron salt is ferrous chloride, and the divalent manganese salt is manganese chloride. The above raw materials are respectively dissolved in deionized water to prepare a mixed metal salt solution.
[0070] Step S2: To a volume of 6.00m 3 Add 2.00m 3deionized water and nitrogen was introduced from the bottom of the reactor, the stirring shaft was turned on and the temperature was raised to 60.00° C., the stirring speed of the stirring shaft was 80.00 rpm, a precipitant, a complexing agent and a chelating agent were added in sequence, the pH of the reaction solution in the reactor was adjusted to 12.00 and the concentration of ammonia water to 6.00 g / L, and a bottom liquid was obtained.
[0071] Step S3, nucleation stage: the stirring speed of the stirring shaft is increased to 370.00rpm, the nitrogen outlet for injecting nitrogen into the reactor is switched from the bottom of the reactor to the top of the reactor and the nitrogen flow rate is maintained at 120.00L / h; a mixed metal salt solution, a precipitant, a complexing agent and a chelating agent are continuously added to the bottom liquid for a co-precipitation reaction, wherein the feed flow rate of the metal salt mixed solution is 50.00L / h, the feed flow rate of the mixed metal salt molten solution, the feed flow rate of the precipitant, the feed flow rate of the complexing agent and the feed flow rate of the chelating agent are 40:15:1:2, and the temperature in the reactor is controlled to be maintained at 60.00±1.00℃, the pH is maintained at 12.00, and the concentration of ammonia water is maintained at 6.00g / L for 2.00h.
[0072] Step S4, passivation stage: the pH in the reactor is reduced to 11.60 at a rate of 0.20 per hour, and the feed flow rate of the mixed metal solution is increased to 75.00 L / h, the feed flow rate of the complexing agent is adjusted according to the ratio of the feed flow rate of the complexing agent to the feed flow rate of the mixed metal salt solution in step S3, and the feed flow rate of the chelating agent is adjusted according to the ratio of the feed flow rate of the chelating agent to the feed flow rate of the mixed metal salt solution in step S3. The temperature in the reactor is controlled to be maintained at 60.00±1.00°C, the pH is maintained at 11.55-11.60, and the concentration of ammonia water is maintained at 5.00 g / L for 10.00 h.
[0073] In step S4, after the reaction liquid in the reactor is full, the mortar pump and the concentrator are turned on to filter the reaction liquid and discharge the filtrate. At the same time, the concentrated liquid is refluxed into the reactor through the reflux pipe to increase the solid content in the reactor and ensure the stability of the liquid level in the reactor and the concentrator.
[0074] Step S5, growth stage: the rotation speed of the stirring shaft is reduced to 250 rpm at a rate of 7.50 rpm per hour, the pH in the reactor is reduced to 11.30 at a rate of 0.05 per hour, the feed flow rate of the complexing agent is reduced to reduce the concentration of the ammonia water in the reactor to 4.00 g / L at a rate of 0.35 g / L per hour, and the feed flow rate of the mixed metal solution is increased to 230.00 L / h, the feed flow rate of the chelating agent is adjusted according to the ratio of the feed flow rate of the chelating agent to the feed flow rate of the mixed metal salt solution in step S3, the temperature in the reactor is controlled to be maintained at 60.00±1.00°C, the pH is maintained at 11.22-11.30, and the concentration of the ammonia water is maintained at 4.00 / L, and the discharge is stopped after 100.00-180.00 hours to obtain a slurry.
[0075] In step S5, the duration of the reaction is confirmed based on the particle size D50 of the material in the slurry, and the particle size of the material is detected. When the particle size D50 of the detected material reaches 7.50 μm and the reaction time of step 5 is within the range of 100.00-180.00 h, the reactor can be stopped and the material can be discharged; if the reaction time has reached 100.00 h and the particle size has not reached 7.50 μm, the reaction is continued for a period of time until the particle size of the material meets the standard and then the reactor is stopped and the material is discharged; if the reaction time has reached 180.00 h, and the particle size has not reached 7.50 μm and the difference with 7.50 μm is within the allowable range (10.00%), the reactor can be stopped in advance and the material can be discharged.
[0076] Step S6, post-processing stage: ageing, washing, drying and sieving the slurry to obtain a sodium ion battery ternary precursor material.
[0077] In step S6, nitrogen is first introduced into the aging tank for protection, and then the slurry in the reactor is put into the aging tank for stirring. The aging lasts for 8-10 hours. The aged slurry is then washed, dried, and sieved to obtain nickel-iron-manganese hydroxide with a particle size of D50=7.50 μm. The obtained nickel-iron-manganese hydroxide is packaged to obtain a finished sodium-ion battery ternary precursor material.
[0078] In order to prevent the chelating agent from decomposing too quickly during the reaction, step S1 also includes diluting hydrazine hydrate and water at a ratio of 1.00:100.00 to prepare a reducing solvent; step S2 also includes adding a reducing solvent to deionized water or deionized water; step S3 also includes continuously adding a reducing solvent to the base liquid; step S4 also includes continuously adding a reducing solvent; step S5 also includes continuously adding a reducing solvent.
[0079] Comparative Example 1
[0080] A method for preparing a ternary precursor material for a sodium ion battery, wherein the steps are the same as those of the method for preparing a ternary precursor material for a sodium ion battery in Example 2, except that in step S1, no sodium gluconate solution is prepared as a chelating agent, in step S2, no chelating agent is added to the base liquid, in step S3, no chelating agent is added to the reactor, in step S4, no chelating agent is added to the reactor, and in step S5, no chelating agent is added to the reactor.
[0081] Comparative Example 2
[0082] A method for preparing a ternary precursor material for a sodium ion battery, wherein the steps are the same as those of the method for preparing a ternary precursor material for a sodium ion battery in Example 3, except that in step S1, a 0.01 mol / L sodium citrate solution is prepared to replace the chelating agent, in step S2, a sodium citrate solution is added to the base liquid to replace the chelating agent, in step S3, a sodium citrate solution is added to the reactor to replace the chelating agent, in step S4, a sodium citrate solution is added to the reactor to replace the chelating agent, and in step S5, a sodium citrate solution is added to the reactor to replace the chelating agent.
[0083] Comparative Example 3
[0084] A method for preparing a ternary precursor material for a sodium ion battery, wherein the steps are the same as those of the method for preparing a ternary precursor material for a sodium ion battery in Example 4, except that the stirring shaft of the reactor used in Comparative Example 3 only has a first stirring component and a third stirring component spaced apart in the vertical direction, and no second stirring component.
[0085] The physical and chemical indicators of the sodium ion battery ternary precursor materials prepared in Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were tested, as shown in Table 1.
[0086] Table 1
[0087]
[0088] Comparing Example 2 with Comparative Example 1, Example 3 with Comparative Example 2, and Example 4 with Comparative Example 3, the sodium ion battery ternary precursor materials prepared in Example 2, Example 3 and Example 4 have better particle size distribution, smaller specific surface area and higher tap density, that is, the sodium ion battery ternary precursor material preparation device provided in Example 1 and the sodium ion battery ternary precursor material preparation method provided in Example 2, Example 3 and the example can prepare a sodium ion battery ternary precursor material with a compact morphology, good sphericity, low activity and high tap density.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a ternary precursor material for a sodium ion battery, characterized in that: The following steps are included: S1, solution preparation stage: use divalent nickel salt solution, divalent iron salt solution and divalent manganese salt solution to prepare a mixed metal salt solution. 2+ , Fe 2+ , Mn 2+ The total molar concentration is 1.50-2.50 mol / L; 6.00-12.00 mol / L sodium hydroxide solution is prepared as a precipitant; 5.00-10.00 mol / L ammonia solution is prepared as a complexing agent; 0.01-0.05 mol / L sodium gluconate solution is prepared as a chelating agent; S2, base liquid preparation stage: in an inert gas atmosphere, add a precipitant, a complexing agent and a chelating agent to pure water or deionized water and stir to obtain a base liquid, the stirring speed is 50.00-100.00 rpm, and the temperature is raised to 50.00-60.00° C. while stirring, the concentration of ammonia water in the base liquid is 3.00-8.00 g / L and the pH of the base liquid is adjusted to 12.00-13.00; S3, nucleation stage: in an inert gas atmosphere, continuously add a mixed metal salt solution, a precipitant, a complexing agent and a chelating agent to the base liquid and stir to perform a co-precipitation reaction, increase the stirring speed to more than 350.00 rpm, and control the pH to be maintained at 12.00-12.30, and the concentration of ammonia water to be maintained at 5.00-8.00 g / L, for 1.00-10.00 h; S4, passivation stage: under an inert gas atmosphere, control the pH to drop to 11.60-11.90, and increase the flow rate of the mixed metal salt solution to 1.50-3.00 times the original flow rate, continue to add the mixed metal salt solution, precipitant, complexing agent and chelating agent and stir, and control the concentration of ammonia water to drop to 3.00-7.00 g / L, and continue for 6.00-20.00 hours; S5, growth stage: under an inert gas atmosphere, control the pH to drop to 11.00-11.60, increase the flow rate of the mixed metal salt solution to 1.50-3.00 times of the original flow rate, continue to add the mixed metal salt solution, precipitant, complexing agent and chelating agent and stir, and the stirring speed is reduced to 200.00-300.00rpm, and the ammonia concentration is reduced to 3.00-6.00g / L, and stop discharging after 30.00-180.00h to obtain slurry; S6, post-processing stage: ageing, washing, drying and screening the slurry to obtain the sodium ion battery ternary precursor material.
2. A method for preparing a ternary precursor material for a sodium ion battery according to claim 1, characterized in that: In step S1, Ni in the mixed metal salt solution 2+ , Fe 2+ , Mn 2+ The molar ratio is x:y:z, wherein x=0.20-0.40, y=0.20-0.40, z=0.20-0.40, and x+y+z=1.
00.
3. A method for preparing a ternary precursor material for a sodium ion battery according to claim 1, characterized in that: In step S1, the divalent nickel salt is one or more of nickel sulfate, nickel nitrate and nickel chloride, the divalent iron salt is one or more of ferrous sulfate, ferrous nitrate and ferrous chloride, and the divalent manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride.
4. A method for preparing a ternary precursor material for a sodium ion battery according to claim 1, characterized in that: In step S4, the pH value decreases at a rate of 0.05-0.20 per hour, and the concentration of ammonia water decreases at a rate of 0.20-0.50 g / L per hour.
5. The method for preparing a ternary precursor material for a sodium ion battery according to claim 1, characterized in that: In step S5, the stirring speed is reduced by 5.00-10.00 rpm per hour, the pH is reduced by 0.05-0.15 per hour, and the concentration of ammonia water is reduced by 0.20-0.50 g / L per hour.
6. A method for preparing a ternary precursor material for a sodium ion battery according to claim 1, characterized in that: Step S1 also includes diluting hydrazine hydrate and water at a ratio of 1.00:100.00 to prepare a reducing solvent; step S2 also includes adding a reducing solvent to pure water or deionized water; step S3 also includes continuously adding a reducing solvent to the base liquid; step S4 also includes continuously adding a reducing solvent; step S5 also includes continuously adding a reducing solvent.
7. A device for preparing ternary precursor materials for sodium ion batteries, characterized in that: A method for preparing a ternary precursor material for a sodium ion battery according to any one of claims 1 to 6, comprising a reactor, a first container, a second container, a third container, a fourth container, a water tank and an inert gas tank, wherein the first container, the second container, the third container, the fourth container, the water tank and the inert gas tank are respectively connected to the reactor, the first container stores a mixed metal salt solution, the second container stores a precipitant, the third container stores a complexing agent, the fourth container stores a chelating agent, the water tank stores pure water or deionized water, and the inert gas tank stores an inert gas.
8. A sodium ion battery ternary precursor material preparation device as claimed in claim 7, characterized in that: It also includes a mortar pump, a temporary storage tank, a concentrator and a reflux pipe. The reactor, mortar pump, temporary storage tank and concentrator are connected in sequence. The reflux pipe connects the concentrator and the reactor to form a loop, and the reflux pipe is provided with a reflux valve for controlling the on-off of the reflux pipe. After the reaction liquid in the reactor is full, the reaction liquid in the reactor is pumped into the temporary storage tank by the mortar pump and flows from the temporary storage tank into the concentrator. The concentrator performs pressure filtration on the reaction liquid and then discharges the filtrate. The concentrated liquid after pressure filtration by the concentrator is refluxed to the reactor through the reflux pipe.
9. A sodium ion battery ternary precursor material preparation device as claimed in claim 7, characterized in that: A rotatable stirring shaft is provided in the reactor, and a first stirring component, a second stirring component and a third stirring component are arranged on the stirring shaft at intervals in the vertical direction. The first stirring component includes a plurality of first stirring blades, and the angle between the first stirring blades and the horizontal plane is 30.00-60.00°. The second stirring component includes a stirring plate and a plurality of second stirring blades arranged on the stirring plate, and the angle between the second stirring blades and the horizontal plane is 45.00°. The third stirring component includes a plurality of third stirring blades, and the angle between the third stirring blades and the horizontal plane is 30.00-60.00°.
10. A sodium ion battery ternary precursor material preparation device as claimed in claim 9, characterized in that: A plurality of baffles are also arranged on the inner wall of the reaction kettle. The baffles extend in a direction close to the stirring shaft and are arranged at intervals along the circumference of the stirring shaft.