A kind of graphene enhanced phenolic resin and coated sand prepared therefrom
By compounding and improving the process of graphene-enhanced phenolic resin, the problem of insufficient heat resistance and mechanical properties of coated sand is solved, and coated sand with high tensile strength and thermal stability is prepared, which is suitable for casting technology.
Patent Information
- Application Number
- CN202311760441.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-12-20
AI Technical Summary
The heat resistance and mechanical properties of existing coated sand are insufficient and cannot meet actual needs.
Using graphene reinforced phenolic resin, through the compounding of carborane phenolic resin and graphene grafted phenolic resin, combined with bisaminosilane coupling agent and polyether polyol, the preparation process of coated sand is improved to improve its strength and thermal stability. stability.
The prepared coated sand has excellent tensile strength and comprehensive mechanical properties, good thermal stability, is suitable for casting technology, and has high practicability.
Smart Images

Figure BDA0004618402370000081 
Figure BDA0004618402370000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coated sand, in particular to a graphene-reinforced phenolic resin and coated sand prepared therefrom. Background Art
[0002] Coated sand was invented by Dr. Kroening of Germany during World War II. The process is to mechanically mix powdered thermosetting phenolic resin with original sand, which solidifies when heated. Later, it gradually developed into coated sand prepared by adding thermoplastic phenolic resin, latent curing agent (urotropine) and lubricant through a certain coating process. When the coated sand is heated, the resin coated on the surface of the sand particles melts, and the coated sand is solidified and formed under the action of urotropine.
[0003] The existing coated sand prepared on the market has poor heat resistance and its mechanical properties cannot meet our actual needs. Therefore, it is necessary to prepare a coated sand with excellent strength and good heat resistance. Summary of the invention
[0004] The object of the present invention is to provide a graphene-enhanced phenolic resin and coated sand prepared therefrom, wherein the graphene-enhanced phenolic resin can be used to prepare coated sand with excellent strength and good heat resistance.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A graphene-enhanced phenolic resin comprises a compound mixture of a carborane phenolic resin and a graphene-grafted phenolic resin, wherein the mass ratio of the carborane phenolic resin to the graphene-grafted phenolic resin is 3:2.
[0007] According to a more optimized scheme, the preparation steps of the carborane phenolic resin are as follows: mix carborane diphenol and isopropanol, stir at 60-65° C. until dissolved, add hydrochloric acid, slowly drop formaldehyde solution, react at 90-100° C. for 12-15 hours, distill under reduced pressure, and dry in vacuum to obtain the carborane phenolic resin.
[0008] In a more optimized solution, the molar ratio of the carborane diphenol to formaldehyde is 1:4; and the amount of hydrochloric acid used is 0.5-1wt% of the carborane diphenol.
[0009] In a more optimized solution, the preparation steps of the graphene-grafted phenolic resin are as follows:
[0010] S1: Mix bisaminosilane coupling agent, ethanol and deionized water, stir until dissolved, add graphene oxide, ultrasonically disperse for 20-30 minutes, stir and react at 60-70°C for 6-8 hours, wash with anhydrous ethanol and deionized water in turn after the reaction, and vacuum dry to obtain functional graphene oxide;
[0011] S2: Mix carborane phenolic resin and epichlorohydrin, stir until dissolved, add sodium hydroxide at 80-85°C, continue to react for 3-4 hours, and perform vacuum distillation to remove unreacted epichlorohydrin to obtain epoxy phenolic resin;
[0012] S3: Mix epoxy phenolic resin and acetone, stir until dissolved, add functional graphene oxide, reflux at 85-90° C. for 3-4 hours, remove acetone under reduced pressure, and obtain graphene-grafted phenolic resin.
[0013] In a more optimized solution, in step S1, the mass ratio of the bisaminosilane coupling agent to the graphene oxide is 10:1; in step S3, the mass ratio of the epoxy phenolic resin to the functional graphene oxide is (7-8):1.
[0014] A more optimized solution is a method for preparing coated sand with graphene enhanced phenolic resin. The preparation steps of the coated sand are: take raw sand, preheat at 180-200°C for 1-1.5h, mix and stir for 5-10min, cool to 120-130°C, add bisaminosilane coupling agent, mix and stir for 3-5min, then heat to 150-160°C, add the graphene enhanced phenolic resin described in any one of claims 1 to 5, 1 / 2 mass of lubricant and polyether polyol, continue to mix for 1-2min, cool to 100-110°C, add curing agent and the remaining 1 / 2 mass of lubricant, mix for 1-2min, discharge, crush and sieve to obtain coated sand.
[0015] In a more optimized solution, the amount of the graphene-enhanced phenolic resin is 3-4wt% of the raw sand, the amount of the polyether polyol is 3-4wt% of the graphene-enhanced phenolic resin, and the bisaminosilane coupling agent is KH-602, and the amount of the bisaminosilane coupling agent is 0.6-0.8wt% of the graphene-enhanced phenolic resin.
[0016] In a more optimized solution, the curing agent is hexamethylenetetramine, and the amount of the curing agent is 13-15wt% of the graphene-enhanced phenolic resin; the lubricant is calcium stearate, and the total amount of the lubricant is 4-6wt% of the graphene-enhanced phenolic resin.
[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0018] The present invention provides a graphene-enhanced phenolic resin, wherein the graphene-enhanced phenolic resin comprises a carborane phenolic resin and a graphene-grafted phenolic resin in an appropriate proportion. The present invention adjusts and improves the preparation process of the carborane phenolic resin, replaces conventional phenol with carborane diphenol, and uses carborane diphenol and formaldehyde as reaction raw materials to react under the action of an acidic catalyst, hydrochloric acid, to generate the carborane phenolic resin. The introduction of the carborane structure can effectively improve the strength and mechanical properties of the coated sand, and the high temperature resistance is also improved, and the product is more practical.
[0019] The present invention further utilizes carborane phenolic resin to be mixed with excess epichlorohydrin, and the hydroxyl groups on the benzene ring react with epichlorohydrin to undergo dehydrochlorination reaction in the presence of sodium hydroxide, thereby introducing epoxy groups with high activity to obtain epoxy phenolic resin. After subsequent curing, the system has high crosslinking density, and the thermal stability and compressive strength of the product can also be improved. At the same time, the present invention grafts a bisaminosilane coupling agent on the surface of graphene oxide, and utilizes the amino groups on the surface of graphene oxide to graft with epoxy phenolic resin to obtain graphene-grafted phenolic resin. The graphene-grafted phenolic resin and the carborane phenolic resin are compounded in a suitable mass ratio, wherein the graphene oxide can play a supporting skeleton role, and can further improve the comprehensive mechanical strength of the coated sand.
[0020] On this basis, the present invention treats the surface of the raw sand with a silane coupling agent, and uses a bisaminosilane coupling agent to modify the raw sand so that the surface of the raw sand contains reactive sites, which promotes the combination between the phenolic resin and the raw sand in the subsequent coating process, and improves the adhesion performance of the two; after the bisaminosilane coupling agent treatment, the graphene-enhanced phenolic resin, lubricant and polyether polyol are added, and the polyether polyol has a large molecular weight and strong polarity, and can be evenly dispersed in the system, thereby improving the toughness and bending strength of the product; after mixing the sand, a curing agent and a lubricant are added, and the material is discharged, crushed and sieved to obtain coated sand. The coated sand has excellent tensile strength and comprehensive mechanical properties, and good thermal stability.
[0021] The invention discloses a graphene-enhanced phenolic resin and coated sand prepared therefrom. The components are reasonably designed, the scheme matching is relatively suitable, the product process steps are simple, and the prepared coated sand has excellent tensile strength and comprehensive mechanical properties, can be applied to casting technology, and has high practicality. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In this embodiment, carborane diphenol is o-carborane bisphenol, provided by Beijing University of Aeronautics and Astronautics; bisaminosilane coupling agent KH-602 and nitrogen aminosilane coupling agent KH-550 are purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; epichlorohydrin is purchased from Tianjin Damao Chemical Reagent Factory; raw sand is 50 / 100 silica sand, purchased from Angnai Molding Sand Factory, Naiman Banner, Inner Mongolia; hexamethylenetetramine and calcium stearate are purchased from Sinopharm Chemical Reagent Co., Ltd.; polyether polyol has a molecular weight of 4000, a hydroxyl value of 26.5-29.5 mg / g, and a viscosity of 800-1000 mPa·s, which is purchased from Shandong Bluestar Dongda Chemical Co., Ltd.
[0024] Graphene oxide was prepared by Hummers method. The specific preparation steps can be referred to "Preparation of phenolic resin / graphene oxide composite materials by in-situ polymerization method".
[0025] Example 1
[0026] The present embodiment provides a graphene-enhanced phenolic resin, wherein the graphene-enhanced phenolic resin comprises a compound mixture of a carborane phenolic resin and a graphene-grafted phenolic resin, and the mass ratio of the carborane phenolic resin to the graphene-grafted phenolic resin is 3:2.
[0027] The preparation steps of the carborane phenolic resin are as follows: 5 mmol of carborane diphenol and isopropanol are mixed, stirred at 60°C until dissolved, hydrochloric acid is added, 20 mmol of formaldehyde solution (the concentration of the formaldehyde solution is 37 wt%) is slowly added dropwise, reacted at 90°C for 15 hours, vacuum distilled, and dried to obtain the carborane phenolic resin. The amount of hydrochloric acid used is 1 wt% of the carborane diphenol.
[0028] The preparation steps of graphene grafted phenolic resin are as follows:
[0029] S1: Take 10g of bisaminosilane coupling agent, 36g of ethanol and 4g of deionized water, mix them, stir until dissolved, add 1g of graphene oxide, ultrasonically disperse for 20min, stir and react at 60°C for 8h, and after the reaction, wash with anhydrous ethanol and deionized water in turn, and vacuum dry to obtain functional graphene oxide; the bisaminosilane coupling agent is KH-602.
[0030] S2: Take 5g of carborane phenolic resin and 36g of epichlorohydrin, mix them, stir until dissolved, add 4g of sodium hydroxide at 80°C, continue to react for 4h, and distill under reduced pressure to remove unreacted epichlorohydrin to obtain epoxy phenolic resin.
[0031] S3: 80 g of epoxy phenolic resin and acetone were mixed and stirred until dissolved, 10 g of functional graphene oxide was added, and refluxed at 85° C. for 4 h. The acetone was removed under reduced pressure to obtain graphene-grafted phenolic resin.
[0032] Example 2
[0033] A graphene-enhanced phenolic resin comprises a compound mixture of a carborane phenolic resin and a graphene-grafted phenolic resin, wherein the mass ratio of the carborane phenolic resin to the graphene-grafted phenolic resin is 3:2.
[0034] The preparation steps of the carborane phenolic resin are as follows: 5 mmol of carborane diphenol and isopropanol are mixed, stirred at 65° C. until dissolved, hydrochloric acid is added, 20 mmol of formaldehyde solution (the concentration of the formaldehyde solution is 37 wt%) is slowly added dropwise, reacted at 100° C. for 12 h, vacuum distilled, and dried in vacuo to obtain the carborane phenolic resin. The amount of hydrochloric acid used is 1 wt% of the carborane diphenol.
[0035] The preparation steps of graphene grafted phenolic resin are as follows:
[0036] S1: Take 10g of bisaminosilane coupling agent, 36g of ethanol and 4g of deionized water, mix them, stir until dissolved, add 1g of graphene oxide, ultrasonically disperse for 30min, stir and react at 70℃ for 6h, wash with anhydrous ethanol and deionized water in turn after the reaction, and vacuum dry to obtain functional graphene oxide; the bisaminosilane coupling agent is KH-602.
[0037] S2: Take 5g of carborane phenolic resin and 36g of epichlorohydrin, mix them, stir until dissolved, add 4g of sodium hydroxide at 85°C, continue to react for 3h, and distill under reduced pressure to remove unreacted epichlorohydrin to obtain epoxy phenolic resin.
[0038] S3: 80 g of epoxy phenolic resin and acetone were mixed and stirred until dissolved, 10 g of functional graphene oxide was added, and refluxed at 90° C. for 3 h. The acetone was removed under reduced pressure to obtain graphene-grafted phenolic resin.
[0039] Example 3
[0040] A graphene-enhanced phenolic resin comprises a compound mixture of a carborane phenolic resin and a graphene-grafted phenolic resin, wherein the mass ratio of the carborane phenolic resin to the graphene-grafted phenolic resin is 3:2.
[0041] The preparation steps of the carborane phenolic resin are as follows: 5 mmol of carborane diphenol and isopropanol are mixed, stirred at 65° C. until dissolved, hydrochloric acid is added, 20 mmol of formaldehyde solution (the concentration of the formaldehyde solution is 37 wt%) is slowly added dropwise, reacted at 95° C. for 14 h, vacuum distilled, and dried in vacuo to obtain the carborane phenolic resin. The amount of hydrochloric acid used is 1 wt% of the carborane diphenol.
[0042] The preparation steps of graphene grafted phenolic resin are as follows:
[0043] S1: Take 10g of bisaminosilane coupling agent, 36g of ethanol and 4g of deionized water, mix them, stir until dissolved, add 1g of graphene oxide, ultrasonically disperse for 30min, stir and react at 65°C for 7h, and after the reaction, wash with anhydrous ethanol and deionized water in turn, and vacuum dry to obtain functional graphene oxide; the bisaminosilane coupling agent is KH-602.
[0044] S2: Take 5g of carborane phenolic resin and 36g of epichlorohydrin, mix them, stir until dissolved, add 4g of sodium hydroxide at 85°C, continue to react for 4h, and distill under reduced pressure to remove unreacted epichlorohydrin to obtain epoxy phenolic resin.
[0045] S3: 80 g of epoxy phenolic resin and acetone were mixed and stirred until dissolved, 10 g of functional graphene oxide was added, and refluxed at 90° C. for 3.5 h. The acetone was removed under reduced pressure to obtain graphene-grafted phenolic resin.
[0046] Example 4
[0047] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 180°C for 1.5h, mix and stir for 5min, cool to 120°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 5min, then heat to 150°C, add 80g of graphene-enhanced phenolic resin prepared in Example 2, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 100°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 48g of carborane phenolic resin and 32g of graphene-grafted phenolic resin, and the bisaminosilane coupling agent is KH-602. The curing agent is urotropine, and the lubricant is calcium stearate.
[0048] Example 5
[0049] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 200°C for 1h, mix and stir for 10min, cool to 130°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 3min, then heat to 160°C, add 80g of graphene-enhanced phenolic resin prepared in Example 2, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 110°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 48g of carborane phenolic resin and 32g of graphene grafted phenolic resin, and the bisaminosilane coupling agent is KH-602. The curing agent is hexamethylenetetramine, and the lubricant is calcium stearate.
[0050] Example 6
[0051] Compared with Example 4, the difference is that the graphene-reinforced phenolic resin prepared in Example 1 is added, and the other processes remain unchanged.
[0052] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 200°C for 1h, mix and stir for 10min, cool to 130°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 3min, then heat to 160°C, add 80g of graphene-enhanced phenolic resin prepared in Example 1, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 110°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 48g of carborane phenolic resin and 32g of graphene grafted phenolic resin, and the bisaminosilane coupling agent is KH-602. The curing agent is hexamethylenetetramine, and the lubricant is calcium stearate.
[0053] Example 7
[0054] Compared with Example 4, the difference is that the graphene-reinforced phenolic resin prepared in Example 3 is added, and the other processes remain unchanged.
[0055] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 180°C for 1.5h, mix and stir for 5min, cool to 120°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 5min, then heat to 150°C, add 80g of graphene-enhanced phenolic resin prepared in Example 3, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 100°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 48g of carborane phenolic resin and 32g of graphene grafted phenolic resin, and the bisaminosilane coupling agent is KH-602. The curing agent is urotropine, and the lubricant is calcium stearate.
[0056] Comparative Example 1
[0057] Compared with Example 4, in Comparative Example 1, no graphene-grafted phenolic resin was added, and only carborane phenolic resin was added, and the rest of the process remained unchanged.
[0058] A method for preparing coated sand by graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 200°C for 1h, mix and stir for 10min, cool to 130°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 3min, then heat to 160°C, add 80g of carborane phenolic resin prepared in Example 2, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 110°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The bisaminosilane coupling agent is KH-602. The curing agent is urotropine, and the lubricant is calcium stearate.
[0059] Comparative Example 2
[0060] Compared with Example 4, in Comparative Example 2, carborane phenolic resin was not added, and only graphene grafted phenolic resin was added, and the rest of the process remained unchanged.
[0061] A method for preparing coated sand by graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 200°C for 1h, mix and stir for 10min, cool to 130°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 3min, then heat to 160°C, add 80g of graphene-grafted phenolic resin prepared in Example 2, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 110°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The bisaminosilane coupling agent is KH-602. The curing agent is urotropine, and the lubricant is calcium stearate.
[0062] Comparative Example 3
[0063] Compared with Example 4, in Comparative Example 3, the carborane phenolic resin and the graphene grafted phenolic resin are compounded in a mass ratio of 1:1, and the other processes remain unchanged.
[0064] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 200°C for 1h, mix and stir for 10min, cool to 130°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 3min, then heat to 160°C, add 80g of graphene-enhanced phenolic resin prepared in Example 2, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 110°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 40g of carborane phenolic resin and 40g of graphene grafted phenolic resin, and the bisaminosilane coupling agent is KH-602. The curing agent is urotropine, and the lubricant is calcium stearate.
[0065] Comparative Example 4
[0066] Compared with Example 4, conventional thermoplastic phenolic resin is used in Comparative Example 4, and the other processes remain unchanged.
[0067] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 200°C for 1h, mix and stir for 10min, cool to 130°C, add 0.64g of bisaminosilane coupling agent, mix and stir for 3min, then heat to 160°C, add 80g of conventional thermoplastic phenolic resin (model 1891, purchased from Shandong Yushiju Chemical Co., Ltd.), 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 110°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 48g of carborane phenolic resin and 32g of graphene-grafted phenolic resin, and the bisaminosilane coupling agent is KH-602. The curing agent is urotropine, and the lubricant is calcium stearate.
[0068] Comparative Example 5
[0069] Compared with Example 4, in Comparative Example 5, only monoaminosilane coupling agent is used, and the other processes remain unchanged.
[0070] A method for preparing coated sand with graphene-enhanced phenolic resin, the specific preparation steps are: take 2kg of raw sand, preheat at 180°C for 1.5h, mix and stir for 5min, cool to 120°C, add 0.64g of monoaminosilane coupling agent, mix and stir for 5min, then heat to 150°C, add 80g of graphene-enhanced phenolic resin prepared in Example 2, 2.4g of lubricant and 3.2g of polyether polyol, continue to mix for 2min, cool to 100°C, add 12g of curing agent and 2.4g of lubricant, mix for 2min, discharge, crush and sieve to obtain coated sand. The graphene-enhanced phenolic resin includes 48g of carborane phenolic resin and 32g of graphene grafted phenolic resin, and the monoaminosilane coupling agent is KH-550. The curing agent is urotropine, and the lubricant is calcium stearate.
[0071] Detection experiment:
[0072] Take the coated sand prepared in Examples 4 to 7 and Comparative Examples 1 to 4, and prepare the molding sand sample according to the standard disclosed in JB / T8834-2001 "Shell (core) phenolic resin for casting", and the specific steps are: place the standard sample mold at 230°C for 1 hour, take it out and pour the coated sand into the mold, the scraper blade is perpendicular to the mold and parallel to the length direction of the mold, scrape the sand from the middle of the sample to both sides twice, press the upper pad after leveling, cure and shape at 230°C, and naturally cool to room temperature after drying to obtain a coated sand "8" shaped standard sand sample with a cross-sectional size of 22.36mm×11.18mm.
[0073] 1. According to JB / T8583-2008 "Coated Sand for Casting", the room temperature tensile strength and room temperature flexural strength are tested; the loading rate of flexural strength is 0.5mm / min.
[0074] 2. Heat resistance: Place the prepared "8"-shaped standard sand sample on a "concave" bracket and place it in a 1000℃ high-temperature furnace to test its collapse time.
[0075] The results are shown in Table 1:
[0076] Table 1
[0077]
[0078]
[0079] As shown in Table 1, when only one of the composite resins is added or the ratio is different from the set ratio, the strength and heat-resistant slump time of the coated sand will be reduced to a certain extent. After adding according to the set ratio, the cold tensile strength of the coated sand is ≥5.5MPa, and the heat-resistant slump time is ≥245s.
[0080] In summary, the components of the present invention are reasonably designed, the scheme ratio is relatively appropriate, the product process steps are simple, and the prepared coated sand has excellent tensile strength and comprehensive mechanical properties, can be applied to casting technology, and has high practicality.
[0081] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A graphene-enhanced phenolic resin, characterized in that: The graphene enhanced phenolic resin comprises a compound mixture of carborane phenolic resin and graphene grafted phenolic resin, wherein the mass ratio of the carborane phenolic resin to the graphene grafted phenolic resin is 3:2; The preparation steps of the carborane phenolic resin are as follows: mixing carborane diphenol and isopropanol, stirring at 60-65° C. until dissolved, adding hydrochloric acid, slowly dropping formaldehyde solution, reacting at 90-100° C. for 12-15 hours, distilling under reduced pressure, and vacuum drying to obtain the carborane phenolic resin; The preparation steps of the graphene-grafted phenolic resin are as follows: S1: Mix bisaminosilane coupling agent, ethanol and deionized water, stir until dissolved, add graphene oxide, ultrasonically disperse for 20-30 minutes, stir and react at 60-70°C for 6-8 hours, wash with anhydrous ethanol and deionized water in turn after the reaction, and vacuum dry to obtain functional graphene oxide; S2: Mix carborane phenolic resin and epichlorohydrin, stir until dissolved, add sodium hydroxide at 80-85°C, continue to react for 3-4 hours, and perform vacuum distillation to remove unreacted epichlorohydrin to obtain epoxy phenolic resin; S3: Mix epoxy phenolic resin and acetone, stir until dissolved, add functional graphene oxide, reflux at 85-90° C. for 3-4 hours, remove acetone under reduced pressure, and obtain graphene-grafted phenolic resin.
2. A graphene-enhanced phenolic resin according to claim 1, characterized in that: The molar ratio of the carborane diphenol to formaldehyde is 1:4; the amount of hydrochloric acid used is 0.5-1wt% of the carborane diphenol.
3. The graphene-enhanced phenolic resin according to claim 1, characterized in that: In step S1, the mass ratio of the bisaminosilane coupling agent to the graphene oxide is 10:1; in step S3, the mass ratio of the epoxy phenolic resin to the functional graphene oxide is (7-8):
1.
4. A method for preparing coated sand by graphene-enhanced phenolic resin, characterized in that: The preparation steps of the coated sand are as follows: take the raw sand, preheat it at 180-200°C for 1-1.5h, mix the sand and stir it for 5-10min, cool it to 120-130°C, add the bisaminosilane coupling agent, mix the sand and stir it for 3-5min, then heat it to 150-160°C, add the graphene-enhanced phenolic resin described in any one of claims 1-3, 1 / 2 of the mass of lubricant and polyether polyol, continue to mix the sand for 1-2min, cool it to 100-110°C, add the curing agent and the remaining 1 / 2 of the mass of lubricant, mix the sand for 1-2min, discharge the material, crush and sieve it, and obtain the coated sand.
5. The method for preparing coated sand by using graphene-enhanced phenolic resin according to claim 4, characterized in that: The amount of the graphene-enhanced phenolic resin is 3-4wt% of the original sand, and the amount of the polyether polyol is 3-4wt% of the graphene-enhanced phenolic resin.
6. The method for preparing coated sand by using graphene-enhanced phenolic resin according to claim 4, characterized in that: The bisaminosilane coupling agent is KH-602, and the amount of the bisaminosilane coupling agent is 0.6-0.8wt% of the graphene-enhanced phenolic resin.
7. The method for preparing coated sand by using graphene-enhanced phenolic resin according to claim 4, characterized in that: The curing agent is hexamethylenetetramine, and the amount of the curing agent is 13-15wt% of the graphene-enhanced phenolic resin; the lubricant is calcium stearate, and the total amount of the lubricant is 4-6wt% of the graphene-enhanced phenolic resin.