An internal and external "double-layer" coupling reinforced TiAl-based composite material and its preparation method

By introducing an internal and external 'double-layer' coupling reinforcement structure into the TiAl-based composite material and utilizing the in-situ self-generation of carbides and borides, the problem of insufficient high-temperature strength of the TiAl-based composite material is solved, and its high-temperature ultimate tensile strength and plasticity, enabling high-performance material preparation.

CN117802341BActive Publication Date: 2024-10-22CHONGQING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410036726.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-10
Publication Date
2024-10-22
Estimated Expiration
2044-01-10

AI Technical Summary

Technical Problem

TiAl-based composite materials have insufficient strength under high temperature conditions of 900°C and above, making it difficult to meet the performance requirements of the aerospace industry. The existing interface layer quasi-continuous network reinforcement structure is limited in improving high-temperature ultimate strength.

Method used

Adopting an internal and external 'double-layer' coupling reinforcement structure, the dispersion reinforcement structure is introduced inside the matrix unit through the in-situ self-generation of carbides, and a quasi-continuous network reinforcement structure is constructed at the interface layer. The in-situ self-generation of boride and carbide is used to synergize Optimize the matrix unit and interface layer structures to prepare high-performance TiAl-based composite materials.

Benefits of technology

The high-temperature ultimate tensile strength and plasticity of TiAl-based composite materials are significantly improved, and a high-performance material with excellent high-temperature strength and plasticity is realized. The mechanical properties of the material are optimized by adjusting the proportion and structure of the reinforcement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117802341B_ABST
    Figure CN117802341B_ABST
Patent Text Reader

Abstract

The present invention discloses an inner-outer "double-layer" coupled reinforced TiAl-based composite material and a preparation method thereof. The composite material comprises an inner layer reinforcement structure and an outer layer reinforcement structure. The inner layer reinforcement structure is composed of in-situ self-generated carbides dispersed in the TiAl matrix unit, and the outer layer reinforcement structure is composed of a quasi-continuous mesh reinforcement structure formed by mixing boride and carbide. The specific method comprises: weighing high-purity titanium sponge, high-purity aluminum, high-purity niobium, and high-purity carbon particles as raw materials, preparing TiAl alloy rods by vacuum induction melting, using the TiAl alloy rods as plasma rotating physical and chemical electrodes to prepare C-enhanced TiAl spherical powders; mixing the spherical TiAl-based composite powders with high-purity B 4 C powder and high-purity carbon powder are put into a ball mill for low-energy ball milling, and a TiAl-based composite material is prepared by spark plasma sintering. The TiAl-based composite material prepared by the present invention can replace nickel-based high-temperature alloys and titanium alloys and be applied to aerospace, military and other fields to meet their lightweight requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an inner-outer "double-layer" coupling-reinforced TiAl-based composite material and a preparation method thereof, belonging to the technical field of advanced preparation of metal-based composite materials. Background Art

[0002] Lightweighting of high-performance structural materials is the key to improving the performance of aerospace engines, extending their life, reducing energy consumption and costs, and directly determines the future sustainable development of the aerospace industry. TiAl-based composite materials have the advantages of low density, high specific strength, excellent oxidation resistance and creep resistance, and their density is about half of that of nickel-based high-temperature alloys. They are the primary candidate materials to replace nickel-based high-temperature alloys to achieve large-scale weight reduction in aerospace engines. The conventional service temperature of nickel-based high-temperature alloys is mostly above 1000°C, but the high-temperature strength of TiAl-based composite materials at 900°C and above is currently difficult to meet the performance requirements of the aerospace industry for high-temperature structural materials. Therefore, achieving a significant improvement in the high-temperature strength and plasticity of TiAl-based composite materials is crucial to promoting their widespread application in the aerospace field.

[0003] In order to improve the mechanical properties of TiAl-based composites, domestic and foreign scholars have introduced quasi-continuous network reinforcement structures into TiAl-based composites, and divided the material organization into matrix units and their interface layer quasi-continuous network reinforcement structures, and conducted extensive research on them. However, the study found that although the interface layer quasi-continuous network reinforcement structure can effectively improve the plasticity of TiAl-based composites, its ability to improve the high-temperature ultimate strength of the material is limited. Therefore, it is necessary to coordinately optimize the design of the material matrix unit and its interface layer quasi-continuous network reinforcement structure. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an inner-outer "double-layer" coupled reinforced TiAl-based composite material, that is, by in-situ self-generation of carbides, a dispersed reinforcement structure ("inner layer" structure) is introduced into the inside of a matrix unit; by in-situ self-generation of borides and carbides, a quasi-continuous network reinforcement structure ("outer layer" structure) is constructed in the interface layer of the matrix unit, and by synergistic optimization of the reinforcement inside the matrix unit and the quasi-continuous network structure of the interface layer, a high-performance TiAl-based composite material with excellent high-temperature strength and plasticity is obtained, which specifically includes the following steps:

[0005] (1) High-purity sponge titanium, high-purity aluminum, high-purity niobium, and high-purity carbon particles are weighed according to atomic percentage, and then a TiAl alloy ingot with a size of φ55 mm×(260-280) mm is prepared by a vacuum induction melting furnace under the protection of an argon atmosphere with a vacuum degree of 0.01-0.05 Pa or 150 mbar, and the oxide scale, oil stains, and impurities on the surface of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×(250-270) mm; finally, the TiAl alloy rod is placed in a rotary clamp of a plasma rotary material-chemical powder making device as an electrode material, and the rotation speed is adjusted to 15000-21000 rpm, the current is 1100-1500 A, and the melting speed is 1.5-3.0 mm·s under the protection of an argon atmosphere. -1 , to prepare C-reinforced TiAl spherical powder.

[0006] (2) Weighing high-purity B4C powder, carbon powder and the spherical TiAl-based composite powder prepared in step (1) as raw materials respectively, and placing the weighed spherical TiAl-based composite powder, high-purity B4C powder and high-purity carbon powder into a ball mill; weighing stainless steel ball milling beads and TiAl powder and B4C powder into the ball mill at a ball-to-material ratio of 5:1 to 2:1; locking the ball mill with a locking device and evacuating the ball mill with a vacuum pump until the air pressure in the ball mill is 10 -2 MPa, stop evacuating, then flush argon into the ball mill until the air pressure of the ball mill is atmospheric pressure, then stop filling argon; put the ball mill into a ball mill, and perform low-energy ball milling for 1 to 10 hours at a ball milling speed of 100 to 300 rpm. It should be noted that the uniformity of the coating of high-purity B4C powder and high-purity carbon powder on the spherical TiAl-based composite powder in step (3) directly determines the distribution of boride and carbide reinforcements in the outer quasi-continuous network reinforcement structure, as well as the integrity and connectivity of the TiAl matrix unit, thereby affecting the comprehensive mechanical properties of the TiAl composite material.

[0007] (3) The ball-milled mixed powder in step (2) is placed in a graphite mold, the mold is placed in a spark plasma sintering furnace, spark plasma sintering is performed at a pressure of 40 to 60 MPa, and the mixture is kept at 1150 to 1300° C. for 5 to 30 minutes, then cooled to room temperature with the furnace, and the mold is taken out after the furnace is opened to obtain a TiAl-based composite material. It should be noted that the sintering temperature and sintering time in step (4) directly determine the type and morphology of the boride and carbide in the inner and outer "double-layer" coupling reinforcement structure, thereby affecting the mechanical properties of the TiAl composite material.

[0008] Preferably, the raw material specifications for preparing the TiAl alloy ingot in step (1) of the present invention are: the particle size of sponge titanium is ≤3 mm, and the purity is ≥99.9wt.%; the particle size of aluminum powder is 6-10 mm, and the purity is ≥99.99wt.%; the particle size of niobium powder is 2-4 mm, and the purity is ≥99.95wt.%; the particle size of carbon particles is ≤0.5 mm, and the purity is ≥99.9wt.%.

[0009] In step (1) of the present invention, the C-reinforced TiAl spherical powder contains, by atomic percentage, 40-50% Al, 2-10% Nb, 0-1% C, and the balance Ti, and the C content is not 0%.

[0010] As a further preferred embodiment of the present invention, the C-reinforced TiAl spherical powder in step (1) of the present invention comprises, by atomic percentage, 43% Al, 6% Nb, 0.5-1% C, and the balance Ti.

[0011] Preferably, the conditions for the plasma rotary chemical powder making of the present invention are: in an argon atmosphere protection environment, the rotation speed is adjusted to 15000-21000rpm, the current is 1100-1500A, and the melting speed is 1.5-3.0mm·s -1, , argon positive pressure 0.05MPa.

[0012] The particle size of the spherical TiAl-based composite powder in step (2) of the present invention is preferably: <75μm, 75-112μm, 112-150μm, 150-250μm and >250μm. The particle size of the TiAl powder directly determines the diameter of the TiAl matrix unit in the sintered tissue, that is, the quasi-continuous network reinforcement structure. The larger the powder particle size, the larger the diameter of the quasi-continuous network structure obtained. In actual production, the proportion of powders in different particle size distribution ranges can be controlled by adjusting the plasma rotating electrode atomization process parameters. According to the powder particle size selection, the double-layer reinforcement structure can also be adjusted according to demand. The particle size of B4C powder is ≤10μm, and the carbon powder is ≤10μm.

[0013] The raw materials and their mass percentage contents in step (2) of the present invention are: 0-10% B4C powder, 0-10% carbon powder and the remainder C-reinforced spherical TiAl-based composite powder, and the contents of B4C powder and carbon powder cannot be zero at the same time.

[0014] As a further preferred embodiment of the present invention, the raw materials and their mass percentage contents in step (2) of the present invention are: 0.1-1.0% of B4C powder and the remainder of C-reinforced spherical TiAl-based composite powder.

[0015] Furthermore, the weight percentage of high-purity B4C powder, high-purity carbon powder and TiAl-based composite powder in step (2) of the present invention determines the content and proportion of boride and carbide reinforcements in the outer quasi-continuous network reinforcement structure of the TiAl-based composite material; the C element content in the spherical TiAl-based composite powder weighed in step (2) determines the content of dispersed carbides in the inner layer reinforcement structure of the TiAl-based composite material matrix unit.

[0016] It should be noted that by adjusting the C element content of the spherical TiAl-based composite powder in step (1) and the weight percentage of the high-purity B4C powder, high-purity carbon powder and spherical TiAl-based composite powder in step (2), the ratio of reinforcements in the inner and outer layer reinforcement structures can be regulated, and the ratio of boride and carbide reinforcements in the outer quasi-continuous network reinforcement structure can be regulated, thereby controlling the overall content and ratio of boride and carbide reinforcements in the TiAl composite material, and ultimately achieving optimal regulation of the mechanical properties of the TiAl composite material.

[0017] It should be noted that by adjusting the particle size of the spherical TiAl-based composite powder weighed in S2, the size, morphology and distribution of the outer quasi-continuous network reinforcement structure can be controlled, thereby achieving optimal regulation of the mechanical properties of the TiAl composite material.

[0018] Another object of the present invention is to provide the inner and outer "double-layer" coupled reinforced TiAl-based composite material, including an inner layer reinforcement structure and an outer layer reinforcement structure, wherein the inner layer reinforcement structure is composed of in-situ autogenous carbides dispersed in the TiAl matrix unit, and the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by a mixture of borides and carbides.

[0019] Furthermore, the in-situ self-generated carbides dispersed inside the TiAl matrix unit of the present invention constitute the inner layer reinforcement structure of the TiAl-based composite material, and the borides and carbides distributed in a quasi-continuous network at the interface layer of the TiAl matrix unit constitute the outer layer reinforcement structure of the TiAl-based composite material. The two are coupled to form an internally and externally controllable "double-layer" coupled reinforcement structure.

[0020] Furthermore, the dispersed carbide reinforcements in the inner layer reinforcement structure of the present invention mainly include TiC, Ti2AlC, Ti3AlC or Ti3AlC2, etc., and the outer layer quasi-continuous network reinforcement structure is mainly composed of borides (TiB or TiB2) and carbides (TiC, Ti2AlC, Ti3AlC or Ti3AlC2, etc.), and the type of reinforcement can be controlled by adjusting the sintering process parameters.

[0021] Furthermore, the content of dispersed carbide reinforcements in the inner layer reinforcement structure of the present invention can be controlled by adjusting the C element content in the TiAl rod during the plasma rotating electrode atomization process, and the content of boride and carbide reinforcements in the outer layer quasi-continuous network reinforcement structure can be controlled by adjusting the content of B4C powder and carbon powder during the ball milling process, ultimately achieving coordinated regulation of the content and proportion of the inner and outer layer reinforcements.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) In the plasma rotating electrode atomization powder making process of the present invention, a TiAl alloy ingot containing C element is prepared by vacuum induction melting technology protected by argon atmosphere, the argon atmosphere prevents oxidation of the material, and the TiAl alloy ingot is melted three times repeatedly to make the composition of the TiAl alloy ingot uniform and the components react completely. After melting, defects such as the oxygen surface layer, impurities and end shrinkage cavities are removed to obtain high-quality TiAl alloy rods; then, the TiAl alloy rod is used as an electrode to prepare a multi-component carbide-reinforced TiAl-based composite powder by plasma rotating electrode atomization, and different types of micron-sized carbide reinforcements are formed in the composite powder by in-situ autogenous reaction of the C element, so as to achieve solid solution of the C element inside the composite powder, significant refinement of the interlamellar spacing and grains, precipitation of micron-sized carbides and good metallurgical bonding with the TiAl matrix, and based on the good self-lubricity and high strength of the carbides, the TiAl-based composite powder is effectively toughened, that is, the matrix unit of the TiAl-based composite material with a "double-layer" coupled reinforcement structure is obtained.

[0024] (2) In the plasma rotating electrode atomization powder making process of the present invention, the stable and controllable heat source of the plasma beam is used to quickly melt the rotating TiAl alloy electrode end, and the molten metal forms a large number of molten droplets under the action of centrifugal force. The molten droplets agglomerate into spheres due to surface tension and condense in an argon atmosphere to form spherical TiAl-based composite powders, thereby avoiding the adhesion of multiple spheres. At the same time, the TiAl-based composite powder particles are formed by the condensation of the molten droplets, and the cooling rate of the molten droplets in the argon atmosphere can reach 10 3 ~10 4 ℃ / s, due to the fast cooling speed, the particle size range of the composite powder formed by atomization is narrow, uniform fine grains and micron-sized carbide reinforcements will be formed in the composite powder. The particle size range of the formed powder can be effectively controlled by adjusting the plasma rotating electrode atomization process parameters.

[0025] (3) The present invention introduces an inner-outer "double-layer" coupled reinforcement structure into the TiAl-based composite material. Through the in-situ self-generation of carbides, a diffuse reinforcement structure ("inner layer" structure) is introduced inside the matrix unit. By utilizing the in-situ self-generation of borides and carbides, a quasi-continuous network reinforcement structure ("outer layer" structure) is constructed in the interface layer of the matrix unit. Among them, the weight percentage of high-purity B4C powder and high-purity carbon powder directly determines the content and proportion of borides and carbides in the outer quasi-continuous network reinforcement structure; the C element content in the spherical TiAl-based composite powder directly determines the carbide content, interlaminar spacing and grain size in the inner layer reinforcement structure of the TiAl matrix unit. Therefore, by adjusting the weight percentage of high-purity B4C powder, high-purity carbon powder and the C element content in the TiAl-based composite powder, the organizational structure of the TiAl matrix unit and the content and proportion of borides and carbides in the "double-layer" reinforcement structure can be synergistically regulated to achieve synergistic strengthening and toughening of the TiAl composite matrix unit and the interface layer, and to prepare high-performance TiAl-based composite materials with excellent high-temperature strength and plasticity. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The SEM image of the appearance morphology of the in-situ self-reinforced TiAl-based composite powder prepared in Example 1;

[0027] Figure 2 The microstructure SEM image of the TiAl-based composite material with a double-layer coupled reinforcement structure prepared in Example 1;

[0028] Figure 3 The SEM image of the appearance morphology of the in-situ self-reinforced TiAl-based composite powder prepared in Example 2;

[0029] Figure 4 The SEM image of the cross-section microstructure of the in-situ self-reinforced TiAl-based composite powder prepared for Example 2;

[0030] Figure 5 The SEM image of the carbide reinforcement in the in-situ self-reinforced TiAl-based composite powder prepared in Example 2;

[0031] Figure 6 The microstructure SEM image of the TiAl-based composite material with a double-layer coupled reinforcement structure prepared in Example 2;

[0032] Figure 7 The microstructure SEM image of the TiAl-based composite material with a double-layer coupled reinforcement structure prepared in Example 3;

[0033] Figure 8 The microstructure SEM image of the TiAl-based composite material with a double-layer coupled reinforcement structure prepared in Example 4;

[0034] Fig. 9 The microstructure SEM image of the TiAl-based composite material with a double-layer coupled reinforcement structure prepared in Example 5;

[0035] Fig.10 SEM image of the microstructure of the TiAl-based alloy with a dispersion-enhanced structure prepared in comparison with Example 1

[0036] Fig.11 The microstructure SEM image of a TiAl-based alloy with a dispersion-enhanced structure prepared for comparison example 2. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to the following contents.

[0038] In the description of the present invention, it should be noted that if no specific conditions are specified in the examples, the experiments are carried out according to conventional conditions or conditions recommended by the manufacturer; if the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0039] Example 1

[0040] A method for preparing an inner-outer "double-layer" coupled reinforced TiAl-based composite material, specifically comprising the following steps:

[0041] (1) Powdering, according to the atomic percentage of 43% Al, 6% Nb, 0.5% C and the balance Ti, high-purity sponge titanium, high-purity aluminum, high-purity niobium, and high-purity carbon particles are weighed as raw materials respectively; then, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×260 mm under the protection of an argon atmosphere environment with a vacuum degree of 0.01-0.05 Pa and a vacuum degree of 150 mbar, and the surface oxide scale, oil stains and impurities of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×250 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making equipment, and the rotation speed is adjusted to 18000 rpm, the current to 1300 A, and the melting speed to 2.5 mm·s under the protection of an argon atmosphere. -1 , TiAl-based composite powder was prepared, and the SEM image of the morphology and microstructure of the TiAl-based composite powder is shown in Figure 1 shown.

[0042] (2) Weighing materials: according to the weight percentage: 0.5% B4C (B4C powder particle size ≤ 10 μm) and the remainder spherical TiAl-based composite powder (particle size 112-150 μm), respectively weigh high-purity B4C powder and the spherical TiAl-based composite powder described in S1 as raw materials.

[0043] (3) Mixing powders: putting the weighed spherical TiAl-based composite powder and high-purity B4C powder into a ball mill; weighing stainless steel ball milling beads according to a ball-to-material ratio of 5:1 and putting them into the ball mill; locking the ball mill and evacuating the ball mill until the air pressure in the ball mill is 10 -2 MPa, and then charge argon into the ball mill until the air pressure in the ball mill reaches atmospheric pressure, then stop charging argon; finally, put the ball mill into a ball mill for low-energy ball milling, with a ball milling speed of 200 rpm and a ball milling time of 1 h.

[0044] (4) Sintering: the milled spherical TiAl-based composite powder and high-purity B4C powder are placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa, and the heating rate is 10°C / min. After being kept at 1250°C for 10 min, the mixture is cooled to room temperature with the furnace. After the furnace is opened, the mold is taken out to obtain a TiAl-based composite material. The SEM image of the microstructure of the TiAl-based composite material is shown in FIG. Figure 2 As shown, reinforcements are precipitated at the interface of the TiAl matrix unit, forming an "outer layer" quasi-continuous network reinforcement structure.

[0045] The inner and outer "double-layer" coupled reinforced TiAl-based composite material described in this embodiment includes an inner layer reinforcement structure and an outer layer reinforcement structure. The inner layer reinforcement structure is composed of in-situ self-generated carbides dispersed in the TiAl matrix unit, and the TiAl-based composite powder forming the matrix unit includes the following components in atomic percentage: 43% Al, 6% Nb, 0.5% C and the remainder Ti; the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by a mixture of borides and carbides, and includes the following components in weight percentage: 0.5% B4C and the remainder spherical TiAl-based composite powder.

[0046] Example 2

[0047] A method for preparing an inner-outer "double-layer" coupled reinforced TiAl-based composite material, specifically comprising the following steps:

[0048] (1) Powdering, according to the atomic percentage of 43% Al, 6% Nb, 1.0% C and the balance Ti, high-purity sponge titanium, high-purity aluminum, high-purity niobium and high-purity carbon particles are weighed as raw materials respectively; then, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×270 mm under the protection of an argon atmosphere environment with a vacuum degree of 0.01-0.05 Pa and a vacuum degree of 150 mbar, and the oxide scale, oil stains and impurities on the surface of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×260 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making equipment, and the rotation speed is adjusted to 18000 rpm, the current to 1300 A and the melting speed to 2.5 mm·s under the protection of an argon atmosphere. -1 , to prepare spherical TiAl-based composite powder; the SEM image of the appearance of the TiAl-based composite powder is shown in Figure 3 The SEM image of the powder cross section microstructure is shown in Figure 4 As shown in the SEM image of the in-situ self-generated carbide in the powder Figure 5 As shown, it can be observed that the TiAl-based composite powder has good sphericity and contains strip-shaped and granular in-situ self-generated carbides.

[0049] (2) Weighing materials: according to the weight percentage: 0.1% B4C (particle size ≤ 10 μm) and the remainder spherical TiAl-based composite powder (particle size 125-250 μm), high-purity B4C powder and the spherical TiAl-based composite powder described in S1 are weighed as raw materials.

[0050] (3) Mixing powders: putting the weighed spherical TiAl-based composite powder and high-purity B4C powder into a ball mill; weighing stainless steel ball milling beads according to a ball-to-material ratio of 5:1 and putting them into the ball mill; locking the ball mill and evacuating the ball mill until the air pressure in the ball mill is 10 -2 MPa, and then charge argon into the ball mill jar until the air pressure in the ball mill jar reaches atmospheric pressure and then stop charging argon; finally, put the ball mill jar into a ball mill for low-energy ball milling, wherein the ball milling speed is 200 rpm and the ball milling time is 1.5 h.

[0051] (4) Sintering: The spherical TiAl-based composite powder and high-purity B4C powder are placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa. The heating rate during sintering is 10°C / min. After keeping at 1250°C for 15 min, the mixture is cooled to room temperature with the furnace. After opening the furnace, the mold is taken out to obtain the TiAl-based composite material.

[0052] The inner layer reinforcement structure of the TiAl matrix unit described in this embodiment is composed of dispersed in-situ autogenous carbides, and the TiAl-based composite powder forming the matrix unit includes the following components in atomic percentage: 43% Al, 6% Nb, 1.0% C and the remainder Ti; the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by a mixture of borides and carbides, and the material includes the following components in weight percentage: 0.1% B4C and the remainder spherical TiAl-based composite powder.

[0053] SEM images of the microstructure of TiAl-based composites Figure 6 As shown, it can be observed that an inner and outer "double-layer" coupled reinforcement structure is formed in the TiAl-based composite material, wherein the dispersed rod-shaped and granular carbides precipitate inside the TiAl matrix unit, forming the "inner layer" reinforcement structure of the material; the in-situ self-generated borides and carbides in the interface layer of the TiAl matrix unit form a quasi-continuous network reinforcement structure, which is the "outer layer" reinforcement structure of the material.

[0054] Example 3

[0055] A method for preparing an inner-outer "double-layer" coupled reinforced TiAl-based composite material, specifically comprising the following steps:

[0056] (1) Powdering, according to the atomic percentage of 43% Al, 6% Nb, 1.0% C and the balance Ti, high-purity sponge titanium, high-purity aluminum, high-purity niobium and high-purity carbon particles are weighed as raw materials respectively; then, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×270 mm under the protection of an argon atmosphere environment with a vacuum degree of 0.01-0.05 Pa and a vacuum degree of 150 mbar, and the oxide scale, oil stains and impurities on the surface of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×260 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making equipment, and the rotation speed is adjusted to 18000 rpm, the current to 1300 A and the melting speed to 2.5 mm·s under the protection of an argon atmosphere. -1 , to prepare spherical TiAl-based composite powder.

[0057] (2) Weighing materials: according to the weight percentage: 0.5% B4C (powder particle size ≤ 10 μm) and the remainder spherical TiAl-based composite powder (particle size 125-250 μm), high-purity B4C powder and the spherical TiAl-based composite powder described in S1 are weighed as raw materials.

[0058] (3) Mixing powders: putting the weighed spherical TiAl-based composite powder and high-purity B4C powder into a ball mill; weighing stainless steel ball milling beads according to a ball-to-material ratio of 5:1 and putting them into the ball mill; locking the ball mill and evacuating the ball mill until the air pressure in the ball mill is 10 -2 MPa, and then argon is charged into the ball mill until the pressure of the ball mill reaches atmospheric pressure; finally, the ball mill is placed in a ball mill for low-energy ball milling, with a ball milling speed of 200 rpm and a ball milling time of 1 h;

[0059] (4) Sintering: The spherical TiAl-based composite powder and high-purity B4C powder are placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa. The heating rate during sintering is 10°C / min. After keeping at 1250°C for 15 min, the mixture is cooled to room temperature with the furnace. After opening the furnace, the mold is taken out to obtain the TiAl-based composite material.

[0060] The inner layer reinforcement structure of the TiAl matrix unit described in this embodiment is composed of dispersed in-situ autogenous carbides, and the TiAl-based composite powder forming the matrix unit includes the following components in atomic percentage: 43% Al, 6% Nb, 1.0% C and the remainder Ti; the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by a mixture of borides and carbides, and the material includes the following components in weight percentage: 0.5% B4C and the remainder spherical TiAl-based composite powder.

[0061] The microstructure SEM images of TiAl-based composites are shown in Figure 2. Figure 7 As shown, it can be found that an internal and external "double-layer" coupled reinforcement structure is formed in the TiAl-based composite material, a dispersed carbide reinforcement is formed inside the TiAl matrix unit, and rod-shaped and granular reinforcements exist in the quasi-continuous network reinforcement structure of the interface layer of the TiAl matrix unit.

[0062] Example 4

[0063] A method for preparing an inner-outer "double-layer" coupled reinforced TiAl-based composite material, specifically comprising the following steps:

[0064] (1) Powdering: according to the atomic percentage of 43% Al, 6% Nb, 1.0% C and the balance Ti, high-purity sponge titanium, high-purity aluminum, high-purity niobium and high-purity carbon particles are weighed as raw materials respectively; then, under the protection of an argon atmosphere with a vacuum degree of 0.05 Pa and 150 mbar, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×270 mm, and the oxide scale, oil stains and impurities on the surface of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×260 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making equipment, and under the protection of an argon atmosphere, the rotation speed is adjusted to 18000 rpm, the current is 1300 A, and the melting speed is 2.5 mm·s -1 , to prepare spherical TiAl-based composite powder.

[0065] (2) Weighing materials: According to the weight percentage: 1.0% B4C (particle size ≤ 10 μm) and the remainder spherical TiAl-based composite powder (particle size 125-250 μm), high-purity B4C powder and the spherical TiAl-based composite powder described in S1 are weighed as raw materials.

[0066] (3) Mixing powders: putting the weighed spherical TiAl-based composite powder and high-purity B4C powder into a ball mill; weighing stainless steel ball milling beads according to a ball-to-material ratio of 5:1 and putting them into the ball mill; locking the ball mill and evacuating the ball mill until the air pressure in the ball mill is 10 -2 MPa, and then charge argon into the ball mill until the air pressure in the ball mill reaches atmospheric pressure, then stop charging argon; finally, put the ball mill into a ball mill for low-energy ball milling, with a ball milling speed of 200 rpm and a ball milling time of 1 h.

[0067] (4) Sintering: The spherical TiAl-based composite powder and high-purity B4C powder are placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa. The heating rate during sintering is 10°C / min. After keeping at 1250°C for 15 min, the mixture is cooled to room temperature with the furnace. After opening the furnace, the mold is taken out to obtain the TiAl-based composite material.

[0068] The inner and outer "double-layer" coupled reinforced TiAl-based composite material described in this embodiment includes an inner layer reinforcement structure and an outer layer reinforcement structure. The inner layer reinforcement structure of the TiAl matrix unit is composed of dispersed in-situ autogenous carbides, and the TiAl-based composite powder forming the matrix unit includes the following components in atomic percentage: 43% Al, 6% Nb, 1.0% C and the remainder Ti; the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by a mixture of borides and carbides, and the material includes the following components in weight percentage: 1.0% B4C and the remainder spherical TiAl-based composite powder.

[0069] SEM images of the microstructure of TiAl-based composites are shown in Figure 2. Figure 8 As shown, it can be observed that an obvious internal and external “double-layer” coupling enhancement structure is formed in the TiAl-based composite material.

[0070] Example 5

[0071] A method for preparing an inner-outer "double-layer" coupled reinforced TiAl-based composite material, specifically comprising the following steps:

[0072] (1) Powdering, according to the atomic percentage of 43% Al, 6% Nb, 1.0% C and the balance Ti, high-purity sponge titanium, high-purity aluminum, high-purity niobium and high-purity carbon particles are weighed as raw materials respectively; then, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×270 mm under the protection of an argon atmosphere environment with a vacuum degree of 0.01-0.05 Pa and a vacuum degree of 150 mbar, and the oxide scale, oil stains and impurities on the surface of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×260 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making equipment, and the rotation speed is adjusted to 18000 rpm, the current to 1300 A and the melting speed to 2.5 mm·s under the protection of an argon atmosphere. -1 , to prepare spherical TiAl-based composite powder.

[0073] (2) Weighing materials: according to the weight percentage: 0.1% B4C (powder particle size ≤ 10 μm) and the remainder spherical TiAl-based composite powder (particle size 95-125 μm), high-purity B4C powder and the spherical TiAl-based composite powder described in S1 are weighed as raw materials.

[0074] (3) Mixing powders: putting the weighed spherical TiAl-based composite powder and high-purity B4C powder into a ball mill; weighing stainless steel ball milling beads according to a ball-to-material ratio of 5:1 and putting them into the ball mill; locking the ball mill and evacuating the ball mill until the air pressure in the ball mill is 10 -2 MPa, and then argon is charged into the ball mill until the pressure of the ball mill reaches atmospheric pressure, and then the argon filling is stopped; finally, the ball mill is placed in a ball mill for low-energy ball milling, wherein the ball milling speed is 200 rpm and the ball milling time is 1 hour;

[0075] (4) Sintering: The spherical TiAl-based composite powder and high-purity B4C powder are placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa. The heating rate during sintering is 10°C / min. After being kept at 1250°C for 5 minutes, the mixture is cooled to room temperature with the furnace. After the furnace is opened, the mold is taken out to obtain the TiAl-based composite material.

[0076] The inner and outer "double-layer" coupled reinforced TiAl-based composite material described in this embodiment includes an inner layer reinforcement structure and an outer layer reinforcement structure. The inner layer reinforcement structure of the TiAl matrix unit is composed of dispersed in-situ autogenous carbides, and the TiAl-based composite powder forming the matrix unit includes the following components in atomic percentage: 43% Al, 6% Nb, 1.0% C and the remainder Ti; the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by a mixture of borides and carbides, and the material includes the following components in weight percentage: 0.1% B4C and the remainder spherical TiAl-based composite powder.

[0077] SEM images of the microstructure of TiAl-based composites Fig. 9 As shown, it can be observed that a quasi-continuous network reinforcement structure is formed at the interface layer of the TiAl matrix unit, and the internal TiAl matrix microstructure is a dual-state structure.

[0078] Comparative Example 1

[0079] A TiAl-based alloy with a dispersion-enhanced structure comprises the following components in atomic percentage: 43% Al, 6% Nb, 0.5% C and the balance Ti. The preparation method thereof comprises the following steps.

[0080] (1) Powdering, according to the atomic percentage of 43% Al, 6% Nb, 0.5% C and the balance Ti, high-purity sponge titanium, high-purity aluminum and high-purity niobium are weighed as raw materials respectively; then, under the protection of an argon atmosphere with a vacuum degree of 0.01-0.05 Pa and 150 mbar, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×270 mm, and the oxide scale, oil stains and impurities on the surface of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×260 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making equipment, and under the protection of an argon atmosphere, the rotation speed is adjusted to 18000 rpm, the current is 1300 A, and the melting speed is 2.5 mm·s -1 , to prepare C-reinforced TiAl spherical powder.

[0081] (2) Sintering: Spherical TiAl-based composite powder (particle size of 112-150 μm) is placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa. The heating rate during sintering is 10°C / min. After keeping at 1250°C for 15 minutes, the powder is cooled to room temperature with the furnace. After opening the furnace, the mold is taken out to obtain a TiAl-based alloy. The ultimate tensile strength of the alloy at 900°C is only 245.5 MPa, and the elongation is only 1.0%.

[0082] The SEM images of the obtained TiAl-based alloy microstructure are shown in Fig.10 As shown, it can be observed that there is no obvious precipitation of carbide or boride reinforcement in the sintered structure, the overall structure presents a uniform dual-state structure, and there are a small number of pores inside the material, and the structure has no obvious double-layer reinforcement structure characteristics.

[0083] Comparative Example 2

[0084] A TiAl-based alloy with a dispersion-enhanced structure comprises the following components in atomic percentage: 43% Al, 6% Nb, 1.0% C and the balance Ti. The preparation method thereof comprises the following steps.

[0085] (1) Powdering: high-purity sponge titanium, high-purity aluminum and high-purity niobium are weighed as raw materials according to the atomic percentage of 43% Al, 6% Nb, 1.0% C and the balance Ti; then, a vacuum induction melting furnace is used to prepare a TiAl alloy ingot with a size of φ55 mm×270 mm under the protection of an argon atmosphere with a vacuum degree of 0.01-0.05 Pa and 150 mbar, and the surface oxide scale, oil stains and impurities of the ingot are removed by mechanical processing to obtain a TiAl alloy rod with a size of φ50 mm×260 mm; finally, the TiAl alloy rod is used as an electrode material and is placed in a rotary clamp of a plasma rotary material-chemical powder making device, and the rotation speed is adjusted to 18000 rpm, the current to 1300 A and the melting speed to 2.5 mm·s under the protection of an argon atmosphere. -1 , TiAl-based composite powder was prepared.

[0086] (2) Sintering: spherical TiAl-based composite powder (particle size of 125-250 μm) is placed in a graphite mold, and the mold is placed in a spark plasma sintering furnace. Spark plasma sintering is performed at a pressure of 50 MPa. The heating rate during sintering is 10°C / min. After being kept at 1250°C for 15 minutes, it is cooled to room temperature with the furnace. After the furnace is opened, the mold is taken out to obtain a TiAl-based alloy. The SEM image of the microstructure of the TiAl-based alloy is shown in FIG. Fig.11 As shown, it can be observed that there are holes in some interface layers between the TiAl matrix in the sintered structure, the matrix structure presents a dual-state structure, a small amount of carbide reinforcement is precipitated, and no double-layer reinforcement structure is formed. The ultimate tensile strength of the alloy at 900°C is only 178.3MPa, and the elongation is less than 2.0%.

[0087] The tensile properties of the TiAl-based composite materials prepared in Examples 1 to 7 were tested at a high temperature of 900° C. The detailed results are shown in Table 1.

[0088] Examples Ultimate tensile strength (MPa) 900℃ elongation (%) Example 1 441.O 2.30 Example 2 253.4 2.52 Example 3 497.3 4.12 Example 4 354.6 3.71 Example 5 251.2 2.26 Comparative Example 1 245.5 1.OO Comparative Example 2 178.3 1.87

[0089] It can be seen from Table 1 that with the design and introduction of the "double-layer" coupling reinforcement structure, the high-temperature ultimate tensile strength and plasticity of the TiAl-based composite material have been significantly improved, especially in Example 3 and Example 4; the experimental results show that due to the solid solution strengthening of the C element, the significant refinement of the interlaminar spacing and grains, the precipitation of micron-sized carbides and the in-situ self-reinforcement formed by their good metallurgical bonding with the TiAl matrix, the strength and hardness of the TiAl-based composite powder prepared by plasma rotating electrode atomization are significantly improved. At the same time, the introduction of the quasi-continuous network reinforcement structure in the matrix unit interface layer, i.e., the "outer layer", helps the connection and diffusion reaction of the TiAl-based composite powder during the sintering process, thereby significantly improving the integrity and connectivity of the reinforced matrix unit in the TiAl-based composite material, and greatly improving the density of the material. In addition, according to the strengthening HS theory of composite material structure design, the "capsule-like" structure formed by the composite material under the action of the quasi-continuous network reinforcement structure helps the strength of the material reach its theoretical limit value, and combined with the carbide dispersion reinforcement structure inside the matrix unit, the synergistic strengthening and toughening of the matrix unit and the interface layer of the TiAl composite material is achieved. In view of this, based on the synergistic strengthening and densification of the "double layer" of the composite material structure, a high-performance TiAl-based composite material with excellent high-temperature strength and plasticity was finally prepared.

Claims

1. A method for preparing an internal and external "double-layer" coupled reinforced TiAl-based composite material, characterized in that: The specific steps include: (1) Sponge titanium, aluminum powder, niobium powder, and carbon particles were weighed according to atomic percentage, and a TiAl alloy ingot was prepared by a vacuum induction melting furnace. The oxide scale, oil stains, and impurities on the surface of the ingot were removed to obtain a TiAl alloy rod. The TiAl alloy rod was used as an electrode material and placed in a rotating fixture of a plasma rotary physical and chemical powder making device. In an argon atmosphere protection environment, a C-reinforced spherical TiAl-based composite powder was prepared; (2) Weighing high-purity B4C powder, carbon powder and the spherical TiAl-based composite powder in step (1) as raw materials, and then ball milling the mixed powders; (3) placing the ball-milled mixed powder in step (2) into a graphite mold, placing the mold into a spark plasma sintering furnace, and performing spark plasma sintering at a pressure of 40 to 60 MPa, the spark plasma sintering temperature is 1150 to 1300° C., and the holding time is 5 to 30 min; after the sintering is completed, cooling to room temperature with the furnace, and removing the mold after opening the furnace to obtain a TiAl-based composite material; The C-reinforced TiAl spherical powder in step (1) comprises, by atomic percentage, 40-50% Al, 2-10% Nb, 0-1% C, and the balance Ti, and the C content is not 0%; The raw materials and their mass percentage contents in step (2) are: 0-10% B4C powder, 0-10% carbon powder and the balance C-reinforced spherical TiAl-based composite powder, and the contents of B4C powder and carbon powder cannot be 0 at the same time; The conditions for plasma rotary pulverization are: in an argon atmosphere protection environment, the rotation speed is adjusted to 15000-21000rpm, the current is 1100-1500A, and the melting speed is 1.5-3.0mm·s -1 , Argon positive pressure 0.05MPa; The particle size distribution of the spherical TiAl-based composite powder in step (2) is respectively <75 μm, 75-112 μm, 112-150 μm, 150-250 μm and >250 μm, the particle size of B4C powder is ≤10 μm, and that of carbon powder is ≤10 μm.

2. The method for preparing the internal and external "double-layer" coupled reinforced TiAl-based composite material according to claim 1, characterized in that: The raw material specifications for preparing the TiAl alloy ingot in step (1) are: the particle size of sponge titanium is ≤3 mm, and the purity is ≥99.9wt.%; the particle size of aluminum powder is 6-10 mm, and the purity is ≥99.99wt.%; the particle size of niobium powder is 2-4 mm, and the purity is ≥99.95wt.%; and the particle size of carbon particles is ≤0.5 mm, and the purity is ≥99.9wt.%.

3. The method for preparing the internal and external "double-layer" coupled reinforced TiAl-based composite material according to claim 1, characterized in that: In step (1), the C-reinforced TiAl spherical powder comprises, by atomic percentage, 43% Al, 6% Nb, 0.5-1% C, and the balance Ti.

4. The method for preparing the internal and external "double-layer" coupled reinforced TiAl-based composite material according to claim 1, characterized in that: The raw materials and their mass percentage contents in step (2) are: 0.1-1.0% of B4C powder and the remainder of C-reinforced spherical TiAl-based composite powder.

5. The method for preparing the internal and external "double-layer" coupled reinforced TiAl-based composite material according to claim 1, characterized in that: In step (3), the low-energy ball milling speed is 100-300 rpm, the ball-to-material ratio is 5:1-2:1, and the ball milling time is 1-10 h.

6. The inner and outer "double-layer" coupled reinforced TiAl-based composite material prepared by the method according to any one of claims 1 to 5, characterized in that: The invention comprises an inner layer reinforcement structure and an outer layer reinforcement structure. The inner layer reinforcement structure is composed of in-situ self-generated carbides dispersed in TiAl matrix units, and the outer layer reinforcement structure is composed of a quasi-continuous network reinforcement structure formed by mixing boride and carbide.