A rare earth magnesium alloy strip / rod for automobile and preparation method thereof
Through the preparation method of rare earth magnesium alloy plate strip/rod, combined with electrical pulse assisted asynchronous rolling and acousto-electrical coupling surface treatment, the problems of deformation ability and surface quality of magnesium alloy at room temperature are solved, and high-efficiency and low-cost production is achieved , suitable for lightweight applications in the automotive field.
Patent Information
- Application Number
- CN202311792214.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-12-25
AI Technical Summary
The existing deformed magnesium alloys have poor deformation ability and low surface quality at room temperature, which leads to limited application in automobiles and other fields. The heating treatment leads to oxidation and high energy consumption, increasing production costs.
The preparation method of rare earth magnesium alloy plate strip/rod material includes smelting, semi-continuous casting, homogenized heat treatment, hot extrusion, electrical pulse assisted asynchronous rolling and annealing process, combined with acoustic and electrical coupling surface treatment, optimize chemical composition to improve The ductility and corrosion resistance of magnesium alloys are used, and the rolling deformation is achieved at room temperature.
The high surface quality and high strength and high plastic properties of rare earth magnesium alloy plate and ribbon are achieved, which reduces production costs and significantly improves the room temperature deformation and corrosion resistance of magnesium alloys, which are suitable for automotive lightweight needs.
Smart Images

Figure CN117802372B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of deformed magnesium alloys, and in particular to a rare earth magnesium alloy plate strip / rod for automobiles and a preparation method thereof. Background Art
[0002] Magnesium alloys have the advantages of high specific strength and specific stiffness, good thermal and electrical conductivity, damping and shock absorption, electromagnetic shielding, easy processing and forming, and easy recycling. They have extremely important application value and broad application prospects in the fields of automobiles, electronic communications, aerospace, and national defense and military, and are known as "green engineering materials in the 21st century". Compared with cast magnesium alloys, deformed magnesium alloys have greater development potential. Through the control of material structure and the application of heat treatment processes, deformed magnesium alloys can obtain higher strength, better ductility and more diverse mechanical properties, thereby meeting the application needs of diversified engineering structural parts. Deformed magnesium alloys often need to be heated to a certain temperature and processed through hot forming technologies such as extrusion, rolling and forging.
[0003] However, due to the close-packed hexagonal structure of magnesium alloys, plastic deformation at room temperature is limited to basal slip and cone twinning, which severely limits the deformation capacity of magnesium alloys at room temperature. Usually, heat treatment is used to improve the deformation capacity of magnesium alloys when preparing deformable magnesium alloys. When the temperature exceeds 225°C, the cylindrical and cone slip systems are activated, and the plastic deformation capacity is greatly improved. However, the stable production of deformable magnesium alloy foil is still difficult to achieve, and frequent heating treatment in the actual production process will cause oxidation of magnesium alloys, while greatly increasing the production cost and energy consumption of magnesium alloys.
[0004] Deformed magnesium alloys are usually used in precision structural parts, which have high requirements for product surface quality. Therefore, how to improve the room temperature deformation ability and surface quality of magnesium alloys has become one of the key issues to be solved in the application field of magnesium alloys. Rare earth elements (RE) have unique extranuclear electron configuration and chemical properties. Adding an appropriate amount of rare earth elements to magnesium alloys can enhance the interatomic bonding force and change the axial ratio of magnesium alloys, which helps to improve the deformation ability of magnesium alloys.
[0005] The Chinese patent application with publication number CN115074588A discloses "a preparation process of a high-strength and plastic rare earth magnesium alloy and a high-strength and plastic rare earth magnesium alloy". The main chemical composition of the rare earth magnesium alloy is: Gd: 5.5-10.5%, Y: 2.5-5.5%, Mn: 0.4-1.0%, Sc: 0.2-0.5%, and the balance is Mg. The rare earth magnesium alloy product has high strength and high plasticity, but fails to solve the problems of poor room temperature deformation, surface quality and corrosion resistance of magnesium alloy.
[0006] The Chinese patent application with publication number CN116837261A discloses "a highly corrosion-resistant magnesium alloy containing aluminum and its preparation method". The chemical composition of the magnesium alloy is: Al: 6-10wt%, Ce: 0.05-1.5wt%, Mn: 0.05-0.5wt%, and the balance is Mg and inevitable impurity elements. Its magnesium alloy product has high corrosion resistance, but it fails to solve the problems of room temperature deformation, poor strength and plasticity, and poor surface quality of magnesium alloy.
[0007] The Chinese patent application with publication number CN114457268A discloses a "space cabin magnesium alloy casting with high surface quality and its casting method". The main chemical composition of the magnesium alloy casting is: Zr: 0.4-0.8%, Zn: 0.1-0.2%, Gd: 10.0-11.0%, Y: 0-3.5%, Si≤0.01%, Al≤0.01%, Fe≤0.01%, and the balance is Mg. It improves the slag inclusion defect of the casting by adding a specific solvent and coating a base film on the surface of the resin sand mold, thereby achieving high surface quality of the casting, but it only involves the surface quality of the magnesium alloy parts, and does not involve the surface quality and room temperature deformation of the magnesium alloy strip. Summary of the invention
[0008] The present invention provides a rare earth magnesium alloy plate / rod for automobiles and a preparation method thereof. The magnesium alloy plate / rod has high surface quality and high strength and high plasticity properties, and the magnesium alloy plate can also achieve large reduction rolling deformation at room temperature, thereby providing reliable technical support for solving the problem of lightweighting of automobiles.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A rare earth magnesium alloy plate / rod for automobiles comprises the following components, measured by mass percentage: Zn 1.0%-10.0%, Al 1.0%-10.0%, Mn 0.5%-5.0%, Si 0.5%-3.0%, RE 0.5%-5.0%; wherein, the Y element accounts for 50%-90% of the RE component, and the rest is one or more of La, Ce, Sm, and Gd, and (Zn+Al) / RE is 1.0-5.0; the balance is Mg and unavoidable impurities.
[0011] Furthermore, the finished product thickness of the rare earth magnesium alloy strip is 0.5 to 1.5 mm, and the finished product diameter of the rare earth magnesium alloy bar is 20 to 80 mm.
[0012] Furthermore, the finished product properties of the rare earth magnesium alloy strip are: yield strength ≥340MPa, tensile strength ≥440MPa, elongation after fracture ≥20%, hydrogen evolution rate ≤0.10mL / cm 2 / day, weight loss rate ≤ 0.10mg / cm 2 / day; The finished product properties of rare earth magnesium alloy bars are: yield strength ≥340MPa, tensile strength ≥440MPa, elongation after fracture ≥20%, and surface roughness Ra ≤30nm.
[0013] A method for preparing rare earth magnesium alloy plates and strips / rods for automobiles. The preparation process of the rare earth magnesium alloy plates and strips includes smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, electric pulse assisted asynchronous rolling and annealing processes; the preparation process of the rare earth magnesium alloy rods includes smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, and acoustic-electric coupling surface treatment processes.
[0014] Furthermore, the preparation of the rare earth magnesium alloy strip includes the following steps:
[0015] 1) Melting; according to the set mass percentage, feed industrial pure magnesium ingots into the crucible, introduce inert gas for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed industrial pure aluminum ingots and industrial pure zinc ingots, and when the furnace temperature rises to 760-800°C, feed Mg-RE master alloy, industrial pure silicon powder, and Mg-Mn master alloy; after all the materials are melted, sprinkle refining agent into the melt for refining, the refining temperature is 760-800°C, and the refining time is 20-40min; and then after slag removal and standing treatment, a magnesium alloy liquid is obtained, the standing temperature is 680-760°C, and the standing time is 30-90min;
[0016] 2) Casting; using a semi-continuous casting process to cast the magnesium alloy liquid, the casting temperature is 680-760° C.; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 100-200 mm; obtaining a magnesium alloy ingot;
[0017] 3) Homogenization heat treatment: placing the magnesium alloy ingot into a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-600°C, and the holding time is 8-12h;
[0018] 4) hot extrusion; placing the magnesium alloy ingot after homogenization heat treatment into an extrusion die, keeping it warm for 30 to 60 minutes and then hot extruding it, the extrusion temperature is 380 to 450 ° C, the extrusion ratio is 20 to 80, the extrusion speed is 5 to 30 mm / s, and a magnesium alloy strip with a thickness of 4 to 10 mm is obtained;
[0019] 5) Electric pulse assisted asynchronous rolling and annealing; the magnesium alloy strip is rolled into shape by electric pulse assisted asynchronous rolling; the rolling speed of the rolling mill is 10-30 m / min, the rolling speed ratio is 1.5-5.0, the rolling passes are 3-15 passes, the rolling reduction rate of a single rolling pass is 0-50%, and the total rolling deformation rate at room temperature is ≥75%; wherein, when the rolling reduction of a single rolling pass is 0, it is the electric pulse assisted annealing process; during electric pulse assisted asynchronous rolling, the electric pulse frequency is 100-2000 Hz, the voltage is 10-100 V, the pulse width is 50-120 μs, and the root mean square current density is 20-120 A / mm 2 ; During electric pulse assisted annealing, the electric pulse frequency is 100-1000Hz, the voltage is 20-70V, the pulse width is 50-120μs, and the root mean square current density is 5-50A / mm 2 , and finally obtain rare earth magnesium alloy strip.
[0020] Furthermore, in step 1), in the Mg-RE master alloy, the mass percentage content of RE is 20% to 50%; in the Mg-Mn master alloy, the mass percentage content of Mn is 10% to 40%.
[0021] Furthermore, in the step 1), the crucible is first preheated at a temperature of 440-600°C; the raw material ingot is first dried at a temperature of 100-200°C; in the step 4), the extrusion die is preheated to 350-380°C before hot extrusion.
[0022] Furthermore, the preparation of the rare earth magnesium alloy rod comprises the following steps:
[0023] 1) Melting; according to the set mass percentage, first feed industrial pure magnesium ingots, introduce inert gas for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed industrial pure aluminum ingots and industrial pure zinc ingots, and when the furnace temperature rises to 760-800°C, feed Mg-RE master alloy, industrial pure silicon powder, and Mg-Mn master alloy; after all the materials are melted, sprinkle refining agent into the melt for refining, the refining temperature is 770-800°C, and the refining time is 20-40min; finally, after slag removal and standing treatment, magnesium alloy liquid is obtained, the standing temperature is 700-760°C, and the standing time is 30-90min;
[0024] 2) Casting; using a semi-continuous casting process to cast the magnesium alloy liquid, the casting temperature is 700-760° C.; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 160-500 mm; obtaining a magnesium alloy ingot;
[0025] 3) Homogenization heat treatment and hot extrusion; the magnesium alloy ingot is placed in a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-550°C, and the holding time is 10-20h; the alloy ingot after homogenization heat treatment is placed in an extrusion die, and hot extrusion is performed after holding for 30-60min, the extrusion temperature is 380-450°C, the extrusion ratio is 10-120, and the extrusion speed is 5-30mm / s, so as to obtain a magnesium alloy rod with a diameter of 20-80mm;
[0026] 4) Acoustic-electric coupling surface treatment; using electric pulse assisted ultrasonic impact surface treatment process, the ultrasonic frequency is 10-50kHz, the ultrasonic amplitude is 5-50μm, the prestress is 100-5000N, the feed rate is 0.01-1.0mm / r, the machine tool spindle speed is 100-1000r / min; the electric pulse frequency is 100-2000Hz, the voltage is 10-100V, the pulse width is 50-120μs; the root mean square current density is 20-120A / mm 2 , and finally obtain rare earth magnesium alloy rods.
[0027] Furthermore, in the step 1), the mass percentage content of RE in the Mg-RE master alloy is 20% to 50%; the mass percentage content of Mn in the Mg-Mn master alloy is 10% to 40%.
[0028] Furthermore, in the step 1), the crucible is first preheated at a temperature of 440-600°C; the raw material ingot is first dried at a temperature of 100-200°C; and in the step 4), the extrusion die is preheated to 350-400°C before hot extrusion.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The chemical composition of the rare earth magnesium alloy strip / rod for automobiles of the present invention is mainly Zn, Al, and RE, and the composition satisfies (Zn+Al) / RE of 1.0 to 5.0. The coordinated application of each element helps to significantly improve the ductility and corrosion resistance of the magnesium alloy. The alloy composition design is simple and the cost is low. Adding an appropriate amount of rare earth elements can not only refine the grains, but also be beneficial to spheroidizing the grains and improving the mechanical properties.
[0031] (2) The present invention adopts smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, electric pulse assisted asynchronous rolling and annealing process to prepare rare earth magnesium alloy cold-rolled strip for automobiles. The process is simple, the operability is strong, and industrial mass production can be realized.
[0032] (3) The present invention adopts electric pulse assisted asynchronous rolling and annealing process to achieve a total deformation rate of magnesium alloy ≥ 75% at room temperature. Compared with the surface oxidation and high energy consumption caused by repeated heating during traditional magnesium alloy hot rolling and annealing, the production cost is effectively reduced; the coupling effect of thermal effect and non-thermal effect brought by electric pulse assisted asynchronous rolling and annealing will introduce additional recrystallization driving force, increase the total recrystallization driving force, and thus improve the grain boundary migration rate and nucleation rate; after cold deformation, the non-uniformity of dislocation density of magnesium alloy will cause local resistivity differences, which will lead to uneven distribution of coupling effect generated by electric pulse in microscopic areas, that is, the selective effect of electric pulse, which promotes preferential nucleation and recrystallization in severe deformation areas such as twins and shear bands. Therefore, the application of electric pulse assisted asynchronous rolling and annealing technology can significantly improve the microstructure of deformed magnesium alloy and thus achieve a significant improvement in the plastic deformation ability of magnesium alloy at room temperature;
[0033] (4) The thickness of the rare earth magnesium alloy strip for automobiles prepared by the present invention is 0.5-1.5 mm, the total rolling deformation rate at room temperature is ≥75%, the yield strength is ≥340 MPa, the tensile strength is ≥440 MPa, the elongation after fracture is ≥20%, and the hydrogen evolution rate is ≤0.10 mL / cm 2 / day, weight loss rate ≤ 0.10mg / cm 2 / day, showing excellent comprehensive properties such as high strength, high plasticity and high corrosion resistance;
[0034] (5) The present invention adopts acoustic-electric coupling surface treatment technology to achieve surface nano-crystallization of rare earth magnesium alloy rods for automobiles; the electric pulse-assisted ultrasonic impact can significantly improve the surface finish (reduce roughness) and hardness of rare earth magnesium alloy rods for automobiles at relatively low temperatures and high strain rates. Increasing the frequency of electric pulse treatment can induce grain refinement through dynamic recrystallization and phase transformation processes, increase the depth of the influence layer of micro-area impact deformation and the microhardness of the impact surface micro-area, thereby improving the surface finish, hardness and wear resistance of rare earth magnesium alloy rods for automobiles;
[0035] (6) The rare earth magnesium alloy rod for automobiles prepared by the present invention has a diameter of 20 to 80 mm, a yield strength of ≥340 MPa, a tensile strength of ≥440 MPa, an elongation after fracture of ≥20%, and a surface roughness of Ra ≤30 nm, showing excellent comprehensive properties such as high strength, high plasticity and high surface quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a microstructure photograph of the rare earth magnesium alloy strip for automobiles prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0037] The rare earth magnesium alloy plate / rod for automobiles described in the present invention comprises the following components by mass fraction: Zn 1.0% to 10.0%, Fe 1.0% to 6.0%, Ag 0.5% to 5.0%, Mn 0.5% to 5.0%, Ca 0.5% to 3.0%, and RE 0.5% to 5.0%; wherein the RE component has Y element as the main element, accounting for 50% to 90%, and the rest is one or more of La, Ce, Sm, and Gd, and (Zn+Al) / RE is 1.0 to 5.0; the remainder is Mg and a small amount of inevitable impurities.
[0038] The rare earth magnesium alloy strip / rod for automobiles described in the present invention includes two products, rare earth magnesium alloy strip and rare earth magnesium alloy rod, and the preparation methods of the two are not exactly the same. Among them, the preparation method of rare earth magnesium alloy strip includes the following processes: smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, electric pulse assisted asynchronous rolling and annealing; the preparation method of rare earth magnesium alloy rod includes the following processes: smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, acoustic-electric coupling surface treatment.
[0039] 1. The preparation method of rare earth magnesium alloy strip for automobiles, the specific steps are as follows:
[0040] 1) Melting: First, preheat the crucible, dry the raw ingots and feed the materials. The preheating temperature of the crucible is 440-600°C. The raw ingots are fully dried at 100-200°C to ensure the purity of the melt after melting. According to the set mass fraction, first feed the industrial pure magnesium ingot, pass in an inert gas (such as Ar gas) for protection and heating and melting; when the furnace temperature reaches 680-730°C, feed the industrial pure aluminum ingot and industrial pure zinc ingot, and when the furnace temperature rises to 760-800°C, feed the Mg-RE master alloy (the mass percentage content of RE is 20%-50%), industrial pure silicon powder, and Mg-RE master alloy (the mass percentage content of RE is 10%-40%). After all the materials are melted, slag removal is required to remove the layer of magnesium oxide and covering agent mixed residue on the surface of the melt. Then sprinkle the refining agent into the melt for refining. The refining temperature is 760-800°C and the refining time is 20-40min. The magnesium alloy liquid can be obtained after slag removal and standing treatment. The standing temperature is 680-760°C and the standing time is 30-90 minutes.
[0041] 2) Casting: The magnesium alloy liquid is cast using a semi-continuous casting process, with a casting temperature of 680-760°C; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 100-200 mm. The ingot needs to be cut into small ingots using a sawing machine. Because the initial ingot surface is rough, the ingot surface needs to be turned and polished.
[0042] 3) Homogenization heat treatment: placing the magnesium alloy ingot into a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-600°C, and the insulation time is 8-12h.
[0043] 4) Hot extrusion; clean the extrusion die, heat the extrusion die to 350-380°C; apply lubricant on the surface of the magnesium alloy ingot that has undergone homogenization heat treatment and put it into the extrusion die, keep it warm for 30-60 minutes and then perform hot extrusion, the extrusion temperature is 380-450°C, the extrusion ratio is 20-80, the extrusion speed is 5-30 mm / s, and a magnesium alloy sheet with a thickness of 4-10 mm is obtained.
[0044] 5) Electric pulse assisted asynchronous rolling and annealing; the magnesium alloy strip is rolled into shape by electric pulse assisted asynchronous rolling, the rolling speed of the rolling mill is 10-30m / min, the rolling speed ratio is 1.5-5.0, the rolling passes are 3-15 passes, the rolling reduction of a single pass is 0-50%, and the total rolling deformation rate at room temperature is ≥75%; wherein, when the rolling reduction of a single pass is 0, it is the electric pulse assisted annealing process; during electric pulse assisted asynchronous rolling, the electric pulse frequency is 100-2000Hz, the voltage is 10-100V, and the pulse width is 50-120μs; the root mean square current density is 20-120A / mm 2 ; During electric pulse assisted annealing, the rolling reduction rate of a single pass is 0, the electric pulse frequency is 100-1000Hz, the voltage is 20-70V, the pulse width is 50-120μs; the root mean square current density is 5-50A / mm 2 .
[0045] Finally, a rare earth magnesium alloy strip with a thickness of 0.5 to 1.5 mm is obtained, with a yield strength of ≥340 MPa, a tensile strength of ≥440 MPa, an elongation after fracture of ≥20%, and a hydrogen evolution rate of ≤0.10 mL / cm 2 / day, weight loss rate ≤ 0.10mg / cm 2 / day, showing excellent comprehensive properties such as high strength, high plasticity and high corrosion resistance.
[0046] 2. The preparation method of rare earth magnesium alloy rod for automobiles, the specific steps are as follows:
[0047] 1) Melting: First, preheat the crucible, dry the raw ingots and feed the materials. The preheating temperature of the crucible is 440-600°C. The raw ingots are fully dried at 100-200°C to ensure the purity of the melt after melting. According to the set mass fraction, first feed the industrial pure magnesium ingot, pass in an inert gas (such as Ar gas) for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed the industrial pure aluminum ingot and industrial pure zinc ingot, and when the furnace temperature rises to 760-800°C, feed the Mg-RE master alloy (the mass percentage content of RE is 20%-50%) and Mg-RE master alloy (the mass percentage content of RE is 10%-40%). After all the materials are melted, slag removal is required to remove a layer of magnesium oxide and covering agent mixed residue on the surface of the melt, and then sprinkle the refining agent into the melt for refining. The refining temperature is 770-800°C and the refining time is 20-40 minutes. The magnesium alloy liquid can be obtained after slag removal and standing treatment. The standing temperature is 700-760°C and the standing time is 30-90 minutes.
[0048] 2) Casting: The magnesium alloy liquid is cast using a semi-continuous casting process, with a casting temperature of 700-760°C; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 160-500 mm. The ingot needs to be cut into small ingots using a sawing machine. Since the initial ingot surface is rough, the ingot surface needs to be turned and polished.
[0049] 3) Homogenization heat treatment and hot extrusion: Put the magnesium alloy ingot into a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-550℃, and the holding time is 10-20h. Clean the extrusion die and heat the extrusion die to 350-400℃; apply lubricant on the surface of the alloy ingot that has undergone homogenization heat treatment and put it into the extrusion die, keep it warm for 30-60min and then perform hot extrusion, the extrusion temperature is 380-450℃, the extrusion ratio is 10-120, the extrusion speed is 5-30mm / s, and a magnesium alloy bar with a diameter of 20-80mm is obtained.
[0050] 4) Acoustic-electric coupling surface treatment; Acoustic-electric coupling surface treatment technology is an electric pulse assisted ultrasonic impact surface treatment process, with an ultrasonic frequency of 10 to 50 kHz, an ultrasonic amplitude of 5 to 50 μm, a prestress of 100 to 5000 N, a feed rate of 0.01 to 1.0 mm / r, and a machine tool spindle speed of 100 to 1000 r / min; an electric pulse frequency of 100 to 2000 Hz, a voltage of 10 to 100 V, a pulse width of 50 to 120 μs, and a root mean square current density of 20 to 120 A / mm 2 .
[0051] Finally, rare earth magnesium alloy bars with a diameter of 20 to 80 mm were obtained, with a yield strength ≥340 MPa, a tensile strength ≥440 MPa, an elongation after fracture ≥20%, and a surface roughness Ra ≤30 nm, showing excellent comprehensive properties such as high strength, high plasticity and high surface quality.
[0052] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0053] [Example]
[0054] Examples 1 to 8 prepare rare earth magnesium alloy plates and strips for automobiles, and Examples 9 to 16 prepare rare earth magnesium alloy bars for automobiles.
[0055] The chemical composition of the rare earth magnesium alloy strip / rod in each embodiment is shown in Table 1, the melting-casting-hot extrusion process parameters of embodiments 1 to 8 are shown in Table 2, the electric pulse assisted rolling process parameters of embodiments 1 to 8 are shown in Table 3, and the electric pulse assisted annealing process parameters and product properties of embodiments 1 to 8 are shown in Table 4. The melting-casting-hot extrusion process parameters of embodiments 9 to 16 are shown in Table 5, and the acoustic-electric coupling surface treatment process parameters and product properties of embodiments 9 to 16 are shown in Table 6.
[0056] Figure 1 This is a microstructure photograph of the rare earth magnesium alloy strip prepared in Example 1.
[0057] Table 1 Chemical composition of rare earth magnesium alloy strips / rods (mass percentage, %)
[0058] Example Zn Al Mn Si RE Y La Ce Sm G (Zn+Al) / RE 1、9 3.23 5.85 1.78 0.82 2.92 2.09 0.28 0.33 0.22 - 3.11 2、10 7.49 4.52 3.45 1.38 3.59 2.45 0.31 - - 0.83 3.35 3、11 4.87 4.09 1.58 1.07 4.75 3.34 - 0.59 0.82 - 1.89 4、12 3.62 3.17 1.25 2.24 2.75 1.85 - 0.64 - 0.26 2.47 5、13 5.81 2.51 1.28 0.89 4.46 3.43 0.77 - 0.26 - 1.87 6、14 6.65 3.70 1.05 1.26 2.36 1.18 - - - 1.18 4.39 7、15 1.44 7.14 2.65 0.71 3.93 2.81 - 1.12 - - 2.18 8、16 9.09 2.49 1.42 2.35 2.87 2.05 - - 0.82 - 4.03
[0059] Table 2 Melting-casting-hot extrusion process parameters for preparing rare earth magnesium alloy strips
[0060]
[0061] Table 3 Process parameters of electric pulse assisted asynchronous rolling for preparing rare earth magnesium alloy strip
[0062]
[0063] Table 4 Electric pulse assisted annealing process parameters and product properties of rare earth magnesium alloy strips
[0064]
[0065] It can be seen from the above embodiments that by adopting the chemical composition design of the present invention, combined with the smelting-casting-homogenization heat treatment-hot extrusion-electric pulse assisted asynchronous rolling and annealing process, a rare earth magnesium alloy strip for automobiles with a thickness of 0.5 to 1.5 mm is finally obtained, with a total rolling deformation of ≥75% at room temperature, a yield strength of ≥340 MPa, a tensile strength of ≥440 MPa, an elongation after fracture of ≥20%, and a hydrogen evolution rate of ≤0.10 mL / cm 2 / day, weight loss rate ≤ 0.10mg / cm 2 / day, showing excellent comprehensive properties such as high strength, high plasticity and high corrosion resistance.
[0066] Table 5 Melting-casting-hot extrusion process parameters for preparing rare earth magnesium alloy bars
[0067]
[0068] Table 6 Acoustic-electric coupling surface treatment process parameters and product properties of rare earth magnesium alloy rods
[0069]
[0070] It can be seen from the above embodiments that by adopting the chemical composition design of the present invention, combined with smelting-casting-homogenization heat treatment and hot extrusion-acoustic-electric coupling surface treatment, a rare earth magnesium alloy bar for automobiles with a diameter of 20 to 80 mm is finally obtained, with a yield strength of ≥340 MPa, a tensile strength of ≥440 MPa, an elongation after fracture of ≥20%, and a surface roughness of Ra ≤30 nm, showing excellent comprehensive properties such as high strength, high plasticity and high surface quality.
[0071] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A rare earth magnesium alloy strip / rod for automobiles, characterized in that: The composition includes the following components in percentage by mass: Zn 3.62% to 10.0%, Al 1.0% to 10.0%, Mn 1.05% to 5.0%, Si 0.5% to 2.35%, and RE 2.36% to 5.0%; wherein, the Y element accounts for 50% to 90% of the RE component, and the rest is one or more of La, Ce, Sm, and Gd, and (Zn+Al) / RE is 1.0 to 5.0; the balance is Mg and unavoidable impurities; the finished product performance of the rare earth magnesium alloy strip is: yield strength ≥340MPa, tensile strength ≥440MPa, elongation after fracture ≥20%, hydrogen evolution rate ≤0.10mL / cm 2 / day, weight loss rate ≤ 0.10mg / cm 2 / day; The finished product properties of rare earth magnesium alloy bars are: yield strength ≥340MPa, tensile strength ≥440MPa, elongation after fracture ≥20%, surface roughness Ra ≤30nm; The preparation of rare earth magnesium alloy strip includes the following steps: 1) Melting; according to the set mass percentage, feed industrial pure magnesium ingots into the crucible, introduce inert gas for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed industrial pure aluminum ingots and industrial pure zinc ingots, and when the furnace temperature rises to 760-800°C, feed Mg-RE master alloy, industrial pure silicon powder, and Mg-Mn master alloy; after all the materials are melted, sprinkle refining agent into the melt for refining, the refining temperature is 760-800°C, and the refining time is 20-40min; and then after slag removal and standing treatment, a magnesium alloy liquid is obtained, the standing temperature is 680-760°C, and the standing time is 30-90min; 2) Casting; using a semi-continuous casting process to cast the magnesium alloy liquid, the casting temperature is 680-760° C.; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 100-200 mm; obtaining a magnesium alloy ingot; 3) Homogenization heat treatment: placing the magnesium alloy ingot into a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-600°C, and the holding time is 8-12h; 4) hot extrusion; placing the magnesium alloy ingot after homogenization heat treatment into an extrusion die, keeping it warm for 30 to 60 minutes and then hot extruding it, the extrusion temperature is 380 to 450 ° C, the extrusion ratio is 20 to 80, the extrusion speed is 5 to 30 mm / s, and a magnesium alloy strip with a thickness of 4 to 10 mm is obtained; 5) Electric pulse assisted asynchronous rolling and annealing; the magnesium alloy strip is rolled into shape by electric pulse assisted asynchronous rolling; the rolling speed of the rolling mill is 10-30 m / min, the rolling speed ratio is 1.5-5.0, the rolling passes are 3-15 passes, the rolling reduction rate of a single rolling pass is 0-50%, and the total rolling deformation rate at room temperature is ≥75%; wherein, when the rolling reduction of a single rolling pass is 0, it is the electric pulse assisted annealing process; during electric pulse assisted asynchronous rolling, the electric pulse frequency is 100-2000 Hz, the voltage is 10-100 V, the pulse width is 50-120 μs, and the root mean square current density is 20-120 A / mm 2 ; During electric pulse assisted annealing, the electric pulse frequency is 100-1000Hz, the voltage is 20-70V, the pulse width is 50-120μs, and the root mean square current density is 5-50A / mm 2 , finally obtaining rare earth magnesium alloy strip; The preparation of rare earth magnesium alloy rods includes the following steps: 1) Melting; according to the set mass percentage, first feed industrial pure magnesium ingots, introduce inert gas for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed industrial pure aluminum ingots and industrial pure zinc ingots, and when the furnace temperature rises to 760-800°C, feed Mg-RE master alloy, industrial pure silicon powder, and Mg-Mn master alloy; after all the materials are melted, sprinkle refining agent into the melt for refining, the refining temperature is 770-800°C, and the refining time is 20-40min; finally, after slag removal and standing treatment, magnesium alloy liquid is obtained, the standing temperature is 700-760°C, and the standing time is 30-90min; 2) Casting; using a semi-continuous casting process to cast the magnesium alloy liquid, the casting temperature is 700-760° C.; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 160-500 mm; obtaining a magnesium alloy ingot; 3) Homogenization heat treatment and hot extrusion; the magnesium alloy ingot is placed in a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-550°C, and the holding time is 10-20h; the alloy ingot after homogenization heat treatment is placed in an extrusion die, and hot extrusion is performed after holding for 30-60min, the extrusion temperature is 380-450°C, the extrusion ratio is 10-120, and the extrusion speed is 5-30mm / s, so as to obtain a magnesium alloy rod with a diameter of 20-80mm; 4) Acoustic-electric coupling surface treatment; using electric pulse assisted ultrasonic impact surface treatment process, the ultrasonic frequency is 10-50kHz, the ultrasonic amplitude is 26-50μm, the prestress is 1102-5000N, the feed rate is 0.01-1.0mm / r, the machine tool spindle speed is 100-1000r / min; the electric pulse frequency is 100-2000Hz, the voltage is 10-100V, the pulse width is 50-120μs; the root mean square current density is 20-120A / mm 2 , and finally obtain rare earth magnesium alloy rods.
2. The rare earth magnesium alloy strip / rod for automobile according to claim 1, characterized in that: The finished product thickness of the rare earth magnesium alloy plate and strip is 0.5 to 1.5 mm, and the finished product diameter of the rare earth magnesium alloy bar is 20 to 80 mm.
3. A method for preparing a rare earth magnesium alloy strip / rod for automobiles as claimed in claim 1 or 2, characterized in that: The preparation process of rare earth magnesium alloy plates and strips includes smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, electric pulse assisted asynchronous rolling and annealing process; the preparation process of rare earth magnesium alloy bars includes smelting, semi-continuous casting, homogenization heat treatment, hot extrusion, acoustic-electric coupling surface treatment process.
4. The method for preparing a rare earth magnesium alloy strip / rod for automobile according to claim 3, characterized in that: The preparation of rare earth magnesium alloy strip includes the following steps: 1) Melting; according to the set mass percentage, feed industrial pure magnesium ingots into the crucible, introduce inert gas for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed industrial pure aluminum ingots and industrial pure zinc ingots, and when the furnace temperature rises to 760-800°C, feed Mg-RE master alloy, industrial pure silicon powder, and Mg-Mn master alloy; after all the materials are melted, sprinkle refining agent into the melt for refining, the refining temperature is 760-800°C, and the refining time is 20-40min; and then after slag removal and standing treatment, a magnesium alloy liquid is obtained, the standing temperature is 680-760°C, and the standing time is 30-90min; 2) Casting; using a semi-continuous casting process to cast the magnesium alloy liquid, the casting temperature is 680-760° C.; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 100-200 mm; obtaining a magnesium alloy ingot; 3) Homogenization heat treatment: placing the magnesium alloy ingot into a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-600°C, and the holding time is 8-12h; 4) hot extrusion; placing the magnesium alloy ingot after homogenization heat treatment into an extrusion die, keeping it warm for 30 to 60 minutes and then hot extruding it, the extrusion temperature is 380 to 450 ° C, the extrusion ratio is 20 to 80, the extrusion speed is 5 to 30 mm / s, and a magnesium alloy strip with a thickness of 4 to 10 mm is obtained; 5) Electric pulse assisted asynchronous rolling and annealing; the magnesium alloy strip is rolled into shape by electric pulse assisted asynchronous rolling; the rolling speed of the rolling mill is 10-30 m / min, the rolling speed ratio is 1.5-5.0, the rolling passes are 3-15 passes, the rolling reduction rate of a single rolling pass is 0-50%, and the total rolling deformation rate at room temperature is ≥75%; wherein, when the rolling reduction of a single rolling pass is 0, it is the electric pulse assisted annealing process; during electric pulse assisted asynchronous rolling, the electric pulse frequency is 100-2000 Hz, the voltage is 10-100 V, the pulse width is 50-120 μs, and the root mean square current density is 20-120 A / mm 2 ; During electric pulse assisted annealing, the electric pulse frequency is 100-1000Hz, the voltage is 20-70V, the pulse width is 50-120μs, and the root mean square current density is 5-50A / mm 2 , and finally obtain rare earth magnesium alloy strip.
5. The method for preparing a rare earth magnesium alloy strip / rod for automobile according to claim 4, characterized in that: In step 1), in the Mg-RE master alloy, the mass percentage content of RE is 20% to 50%; in the Mg-Mn master alloy, the mass percentage content of Mn is 10% to 40%.
6. The method for preparing a rare earth magnesium alloy strip / rod for automobile according to claim 4, characterized in that: In the step 1), the crucible is first preheated at a temperature of 440-600° C.; the raw material ingot is first dried at a temperature of 100-200° C.; in the step 4), the extrusion die is preheated to 350-380° C. before hot extrusion.
7. The method for preparing rare earth magnesium alloy strip / rod for automobile according to claim 3, characterized in that: The preparation of rare earth magnesium alloy rods includes the following steps: 1) Melting; according to the set mass percentage, first feed industrial pure magnesium ingots, introduce inert gas for protection and heat to melt; when the furnace temperature reaches 680-730°C, feed industrial pure aluminum ingots and industrial pure zinc ingots, and when the furnace temperature rises to 760-800°C, feed Mg-RE master alloy, industrial pure silicon powder, and Mg-Mn master alloy; after all the materials are melted, sprinkle refining agent into the melt for refining, the refining temperature is 770-800°C, and the refining time is 20-40min; finally, after slag removal and standing treatment, magnesium alloy liquid is obtained, the standing temperature is 700-760°C, and the standing time is 30-90min; 2) Casting; using a semi-continuous casting process to cast the magnesium alloy liquid, the casting temperature is 700-760° C.; the ingot pulling speed is 120-180 mm / min, and the crystallizer diameter is 160-500 mm; obtaining a magnesium alloy ingot; 3) Homogenization heat treatment and hot extrusion; the magnesium alloy ingot is placed in a heating furnace for homogenization heat treatment, the heating furnace temperature is 450-550°C, and the holding time is 10-20h; the alloy ingot after homogenization heat treatment is placed in an extrusion die, and hot extrusion is performed after holding for 30-60min, the extrusion temperature is 380-450°C, the extrusion ratio is 10-120, and the extrusion speed is 5-30mm / s, so as to obtain a magnesium alloy rod with a diameter of 20-80mm; 4) Acoustic-electric coupling surface treatment; using electric pulse assisted ultrasonic impact surface treatment process, the ultrasonic frequency is 10-50kHz, the ultrasonic amplitude is 26-50μm, the prestress is 1102-5000N, the feed rate is 0.01-1.0mm / r, the machine tool spindle speed is 100-1000r / min; the electric pulse frequency is 100-2000Hz, the voltage is 10-100V, the pulse width is 50-120μs; the root mean square current density is 20-120A / mm 2 , and finally obtain rare earth magnesium alloy rods.
8. The method for preparing rare earth magnesium alloy strip / rod for automobile according to claim 7, characterized in that: In the step 1), the mass percentage content of RE in the Mg-RE master alloy is 20% to 50%; the mass percentage content of Mn in the Mg-Mn master alloy is 10% to 40%.
9. The method for preparing rare earth magnesium alloy strip / rod for automobile according to claim 7, characterized in that: In the step 1), the crucible is first preheated at a temperature of 440-600° C.; the raw material ingot is first dried at a temperature of 100-200° C.; in the step 4), the extrusion die is preheated to 350-400° C. before hot extrusion.
Citation Information
Cited By
High-performance fine-grain magnesium alloy and preparation method thereof
CN121718775A