Glass products with transition layers and their preparation methods, and methods for observing the transition layers in glass products.
By applying pressure and heat treatment to glass products to form a uniform transition layer, the problems of thin transition layers and difficulty in observation are solved, thereby improving the shatter resistance and production efficiency of glass products and providing an effective observation method.
Patent Information
- Application Number
- CN202211197188.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-09-29
AI Technical Summary
In the prior art, the transition layer of glass products is too thin and uneven, which leads to stress concentration, making them easy to break, and there is a lack of methods for observing the transition layer of colored glass.
After cleaning, the first and second glass surfaces are brought into contact and subjected to point pressure treatment to remove the air layer between the contact surfaces. Then, heat treatment is performed to form a clear and uniform transition layer, and the thickness of the transition layer is observed using the inclined grinding method.
A transition layer of uniform thickness was prepared, which reduced stress concentration, improved production efficiency, and provided an intuitive method for observing the transition layer, thus reducing the risk of breakage.
Smart Images

Figure CN117819809B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of glass manufacturing technology, specifically to a glass product with a transition layer, its preparation method, and a method for observing the transition layer in the glass product. Background Technology
[0002] Glass welding technology has been successfully applied to both functional and decorative components, such as camera protective covers, integrated frame covers, and logo protective covers.
[0003] CN110790517A discloses a housing, its manufacturing method, a display device, and a terminal device. The method for manufacturing the housing includes: cleaning at least a portion of the surfaces of a first glass element and at least a portion of the surfaces of a second glass element to form clean surfaces; activating the clean surfaces of the first and second glass elements respectively using an alkaline activating solution to form activated surfaces; and bringing the activated surfaces of the first and second glass elements into contact, thereby bonding the first and second glass elements together to obtain the housing.
[0004] Existing processes produce glass products with extremely thin or unevenly distributed transition layers, which can easily cause stress concentration in the product itself, making it prone to breakage during subsequent processing. Moreover, the transition layer has a crucial impact on the integrated glass after fusion, but existing technologies rarely study methods for glass transition layers. Observation of transition layers in colored glass has also not been addressed. Summary of the Invention
[0005] The purpose of this invention is to overcome the problems of excessively thin transition layers in glass products and the lack of observation methods for colored glass transition layers in existing technologies, and to provide a glass product with a transition layer, its preparation method, and an observation method for the transition layer in the glass product.
[0006] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a glass article with a transition layer, wherein the method includes: cleaning, combining and heat-treating a first glass and a second glass to obtain a glass article with a transition layer;
[0007] The combination involves bringing the cleaned first and second glass into contact and applying pressure to remove the air layer between the contact surfaces of the first and second glass.
[0008] A second aspect of the present invention provides a glass article having a transition layer obtained by the aforementioned preparation method.
[0009] A third aspect of the present invention provides a method for observing a transition layer in a glass article, wherein the first glass and the second glass in the glass article are of different colors, and the observation method includes the following steps:
[0010] (1) Grind the glass product at an angle α to expose the entire transition layer;
[0011] (2) Measure the width y of the exposed transition layer;
[0012] (3) The thickness of the transition layer x is calculated by x = y·sinα.
[0013] The beneficial technical effects achieved by the present invention through the above technical solution are as follows:
[0014] (1) This invention produces glass products with a distinct transition layer. The thickness of the transition layer is increased compared to existing technologies, and its distribution is more uniform, reducing stress concentration and making it less prone to breakage during subsequent processing. In addition, the preparation method described in this invention can shorten the production cycle and greatly improve production efficiency.
[0015] (2) The observation method of the transition layer in glass products provided by the present invention can directly see the transition layer and obtain the thickness value of the transition layer. Attached Figure Description
[0016] Figure 1 This is a flowchart of the preparation method of the glass article with a transition layer according to the present invention;
[0017] Figure 2 This is a schematic diagram illustrating the conversion principle for testing the transition layer of colored glass products.
[0018] Figure 3 This is a finished product image of Example 3;
[0019] Figure 4a This is a grinding sample diagram from Example 3;
[0020] Figure 4b These are micrographs of Example 3;
[0021] Figure 5a This is a micrograph of the cross-section of the glass product obtained in Example 3;
[0022] Figure 5b The polarizer of the glass product obtained in Example 3 is shown in the figure;
[0023] Figure 6a This is a micrograph of the cross-section of the glass product obtained in Comparative Example 1.
[0024] Figure 6b This is a schematic diagram of the stress distribution of the glass product sample obtained in Comparative Example 1 using a polarizer. Detailed Implementation
[0025] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0026] The first aspect of the present invention provides a method for preparing a glass article with a transition layer, wherein the method includes: cleaning, combining and heat-treating a first glass and a second glass to obtain a glass article with a transition layer;
[0027] The assembly process includes bringing the cleaned first and second glass into contact and applying point pressure to remove the air layer between the contact surfaces of the first and second glass.
[0028] In this invention, the air layer between the contact surfaces of a first glass and a second glass, cleaned and free of solution, is removed by applying point pressure. Alternatively, the cleaned glass can be air-dried or dried using other methods to obtain the first and second glass surfaces free of solution. The principle of the assembly method described in this invention is to press the combined glass together tightly through point pressure treatment, ensuring the spacing between the surfaces meets the requirements for the interaction of reactive groups—silanol groups. This results in a glass product with a distinct transition layer, significantly shortening the production cycle and improving production efficiency. The thickened transition layer provides more stress release space, reduces stress concentration, makes subsequent processing less prone to breakage, and improves impact resistance.
[0029] In this invention, a rod with a diameter of 3-10mm that will not scratch the glass can be used for point pressurization. This invention employs point pressurization to utilize the glass's own hydroxyl groups to adsorb water layers, relying on atmospheric pressure to evenly expel the air layer and prevent trapped air.
[0030] In this invention, a material preparation step can be added before the cleaning step, and a decoration processing step can be added after the heat treatment step. The material preparation step and the decoration processing step can be performed using commonly used techniques in the prior art.
[0031] In some embodiments of the present invention, the pressurization is point pressurization. Point pressurization in this invention involves selecting at least one point on the combined contact surface of the first and second glass panes and applying pressure until the air layer between the contact surfaces is completely removed. Whether the air layer has been completely removed can be determined by visual inspection; if it is not completely removed, an iridescent phenomenon will occur.
[0032] In some preferred embodiments of the present invention, the pressure applied at the point is 0.05-5 MPa, for example, 0.05 MPa, 0.5 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, or any value within the range of any two of the above values, preferably 0.1-3 MPa. In this invention, controlling the pressure applied at the point within a specific range allows for better assembly of the glass; excessive pressure will cause the glass to shatter, while insufficient pressure will prevent the self-assembly effect from being triggered.
[0033] In some preferred embodiments of the present invention, before the combination, the flatness of the first glass and the second glass is 0.001-0.05 μm, for example 0.001 μm, 0.005 μm, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, and any value within the range of any two of the above values, preferably 0.01-0.03 μm. In the present invention, limiting the flatness of the first glass and the second glass to a specific range before combination can better induce the self-combining effect.
[0034] In some preferred embodiments of the present invention, before the combination, the surface roughness of the first glass and the second glass is 0.01-1 nm, for example, 0.01 nm, 0.05 nm, 0.1 nm, 0.3 nm, 0.5 nm, 1 nm, and any value within the range of any two of the above values, preferably 0.2-0.4 nm. In the present invention, limiting the surface roughness of the first glass and the second glass to a specific range before combination can prevent the undesirable phenomenon of air entrapment caused by unevenness.
[0035] In some embodiments of the present invention, the heat treatment includes sequential heating, holding, and cooling.
[0036] During the heat treatment process, a large number of silanol groups in the hydration layer with a thickness of about 0.1-20μm participate in the chain reaction at high temperature, making two or more pieces of glass become an integrated glass, and the hydration layer is transformed into a transition layer.
[0037] In some preferred embodiments of the present invention, the heating rate is 0.5-20℃ / min, for example 0.5℃ / min, 1℃ / min, 3℃ / min, 5℃ / min, 8℃ / min, 12℃ / min, 15℃ / min, 18℃ / min, 20℃ / min, and any value within any range of any two of the above values, preferably 5-10℃ / min. In the present invention, excessively rapid heating can cause cracking at the assembly point or induce a large number of bubbles on the assembly surface; excessively slow heating leads to low production efficiency.
[0038] In some preferred embodiments of the present invention, the insulation temperature is 300-700℃, for example, any value within the range of any two of the above values, preferably 500-650℃. In the present invention, if the insulation temperature is too low, the combined glass cannot be fully integrated, and loose connections are likely to occur; if the insulation temperature is too high, the combined glass will deform, and pitting will appear on the surface.
[0039] In some preferred embodiments of the present invention, the heat preservation time is 1-60 minutes, for example, 1 minute, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes, or any value within any range of two of the above values, preferably 10-30 minutes. In the present invention, if the heat preservation time is too short, a loose connection may easily occur; if the heat preservation time is too long, the combined glass may easily deform.
[0040] In some preferred embodiments of the present invention, the cooling rate is 1-30℃ / min, for example 1℃ / min, 3℃ / min, 5℃ / min, 8℃ / min, 12℃ / min, 15℃ / min, 18℃ / min, 20℃ / min, 25℃ / min, 30℃ / min, and any value within the range of any two of the above values, preferably 8-15℃ / min. In the present invention, if the cooling is too rapid, the glass will shatter; if the cooling is too slow, production efficiency will be low, and production energy will be wasted.
[0041] In some preferred embodiments of the invention, the heat treatment is performed without pressure. This lack of pressure not only reduces the internal stress of the integrated glass but also lowers production energy consumption, making it more environmentally friendly, reducing equipment requirements, and lowering production costs.
[0042] In some embodiments of the present invention, the preparation method further includes: performing surface treatment on the cleaned first glass and the second glass before the combination.
[0043] In this invention, the purpose of surface treatment is to increase the number of reactive groups - silanol groups - on the glass surface and adsorb a large number of water molecules to protect the activity of silanol groups, which is beneficial to extend the storage time and improve the yield of subsequent heat treatment, and reduce the poor interfacial gap caused by insufficient activity due to insufficient silanol groups or adsorption of other impurities.
[0044] In some preferred embodiments of the present invention, the surface treatment is selected from at least one of alkaline treatment, acid treatment and plasma treatment, preferably alkaline treatment.
[0045] In some embodiments of the present invention, the alkaline treatment process includes immersing the cleaned first and second glass in a first alkaline treatment solution for a first ultrasonic treatment, and then immersing them in a second alkaline treatment solution for a second ultrasonic treatment. In the present invention, the hydration layer formed by the alkaline treatment is dense and thick, which can greatly reduce the wetting angle of the glass surface, while effectively protecting the main reactive group - silanol groups.
[0046] In some preferred embodiments of the present invention, the first alkaline treatment solution comprises, by mass percentage: 1-10% alkali, 0.1-5% triethanolamine, 0.1-3% alkaline salt, 0.05-1% sodium dodecylbenzenesulfonate, 0.1-5% fatty alcohol polyoxyethylene ether, and 76-97.4% H2O.
[0047] In this invention, the alkali in the first alkaline treatment solution reacts with the glass, increasing the amount of silicon-oxygen ring-opening. Furthermore, the glass surface itself has a subsurface layer approximately 1 μm thick, possessing high activity and porous characteristics, containing a certain amount of broken bonds. It also adsorbs other substances. Alkaline treatment can re-process these broken bonds, stripping away the previously adsorbed substances, resulting in a significant increase in the number of broken bonds. After bond breaking and ring opening, E-groups [SiO4] are generated. - and D group [SiO3] + In an alkaline environment, the D group not only absorbs water molecules, but also absorbs OH- ions from the solution. - Since hydroxide ions are polar covalent bonds, they are more likely to adsorb water molecules. In addition, E and D groups will also react with adsorbed water molecules to form silanol groups, i.e., -Si-OH, which will also adsorb water molecules.
[0048] In some preferred embodiments of the present invention, the alkali is sodium hydroxide and / or potassium hydroxide.
[0049] In some preferred embodiments of the present invention, the alkaline salt is sodium carbonate and / or potassium carbonate.
[0050] In some preferred embodiments of the present invention, the temperature of the first ultrasonic treatment is 25-90°C, for example, any value within the range of any two of the above values, preferably 45-70°C. In the present invention, limiting the temperature of the first ultrasonic treatment to a specific range ensures that the effect is achieved in a short time while preventing the volatilization and decomposition of the alkali solution.
[0051] In some preferred embodiments of the present invention, the duration of the first ultrasonic treatment is 1-10 minutes, for example, any value within the range of any two of the above values, preferably 3-5 minutes. In the present invention, limiting the duration of the first ultrasonic treatment to a specific range ensures that the effect is achieved in a short time, saving production resources.
[0052] In some preferred embodiments of the present invention, the frequency of the first ultrasonic treatment is 1000-8000Hz, for example, any value within the range of any two of the above values, preferably 3000-6000Hz. In the present invention, limiting the frequency of the first ultrasonic treatment to a specific range allows for a more regular and uniform distribution of the hydration layer.
[0053] In some preferred embodiments of the present invention, the second alkaline treatment solution is an alkaline solution with a mass percentage of 1-10%.
[0054] In some preferred embodiments of the present invention, the alkali in the alkaline solution is sodium hydroxide and / or potassium hydroxide.
[0055] In some preferred embodiments of the present invention, the temperature of the second ultrasonic treatment is 25-90°C, or any value within the range of any two of the above values, preferably 45-70°C. In the present invention, limiting the temperature of the second ultrasonic treatment to a specific range ensures that the effect is achieved in a short time while preventing the evaporation of the alkali solution.
[0056] In some preferred embodiments of the present invention, the time for the second ultrasonic treatment is 1-10 minutes, or any value within the range of any two of the above values, preferably 3-5 minutes. In the present invention, limiting the time of the second ultrasonic treatment to a specific range ensures that the effect is achieved in a short time, saving production resources.
[0057] In some preferred embodiments of the present invention, the frequency of the second ultrasonic treatment is 1000-8000 Hz, or any value within the range of any two of the above values, preferably 3000-6000 Hz. In the present invention, limiting the frequency of the second ultrasonic treatment to a specific range allows the glass surface to be hydroxylated as much as possible.
[0058] In some embodiments of the present invention, the acid treatment process includes immersing the cleaned first glass and second glass in a first acidic treatment solution for a third ultrasonic treatment, and then immersing them in a second acidic treatment solution for a fourth ultrasonic treatment.
[0059] In some preferred embodiments of the present invention, the first acidic treatment solution comprises, by mass percentage: 1-5% HF, 1-10% H3PO4, 0.5%-10% HNO3 and 75-97.25% H2O.
[0060] In some preferred embodiments of the present invention, the second acidic treatment solution is an acid solution with a mass percentage of 1-10%.
[0061] In some preferred embodiments of the present invention, the acid in the acid solution is hydrochloric acid.
[0062] In this invention, the HF in the first acidic treatment solution can clean and corrode the glass surface, removing the subsurface layer of the glass, increasing the relative surface area of the glass, and combining with H3PO4 and HNO3 to form a large number of broken silicon-oxygen bonds and silicon-silicon bonds, forming E groups [SiO4]. - and D group [SiO3] + A large amount of H exists in acidic environments. + It combines with some E groups. In addition, E and D groups also react with adsorbed water molecules to form silanol groups and adsorb water molecules. Under the further action of HCl, these two groups continue to transform into silanol groups. The -OH group bound in the acidic environment is neutral, and fewer water molecules are adsorbed.
[0063] In some preferred embodiments of the present invention, the temperature of the third ultrasonic treatment is 15-40°C, for example, 15°C, 18°C, 20°C, 22°C, 25°C, 30°C, 35°C, 40°C, and any value within any range of two of the above values, preferably 20-30°C. In this invention, limiting the temperature of the third ultrasonic treatment to a specific range can ensure the effectiveness while preventing acid evaporation and protecting the safety of equipment and operators.
[0064] In some preferred embodiments of the present invention, the time for the third ultrasonic treatment is 1-30s, for example 1s, 5s, 10s, 15s, 20s, 25s, 30s, and any value within the range of any two of the above values, preferably 5-15s. In the present invention, limiting the time of the third ultrasonic treatment to a specific range can ensure the flatness and roughness of the glass while removing microcracks.
[0065] In some preferred embodiments of the present invention, the frequency of the third ultrasonic treatment is 1000-5000Hz, such as 1000Hz, 1200Hz, 1500Hz, 1800Hz, 2000Hz, 2500Hz, 3000Hz, 3500Hz, 4000Hz, 4500Hz, 5000Hz, and any value within any range of two of the above values, preferably 2000-3000Hz. In the present invention, limiting the frequency of the third ultrasonic treatment to a specific range can accelerate the reaction speed, increase the bond breaking speed, and remove microcracks.
[0066] In some preferred embodiments of the present invention, the temperature of the fourth ultrasonic treatment is 15-40°C, for example, 15°C, 18°C, 20°C, 22°C, 25°C, 30°C, 35°C, 40°C, and any value within any range of two of the above values, preferably 20-30°C. In the present invention, limiting the temperature of the fourth ultrasonic treatment to a specific range ensures that microcracks are removed while bonds are broken.
[0067] In some preferred embodiments of the present invention, the duration of the fourth ultrasonic treatment is 2-6 minutes, for example, 2 minutes, 2.2 minutes, 2.5 minutes, 3 minutes, 3.3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, 5.5 minutes, 6 minutes, and any value within any range of two of the above values, preferably 3-5 minutes. In the present invention, limiting the duration of the fourth ultrasonic treatment to a specific range allows for sufficient hydroxylation of the glass surface.
[0068] In some preferred embodiments of the present invention, the frequency of the fourth ultrasonic treatment is 1000-5000Hz, for example, 1000Hz, 1200Hz, 1500Hz, 1800Hz, 2000Hz, 2500Hz, 3000Hz, 3500Hz, 4000Hz, 4500Hz, 5000Hz, and any value within the range of any two of the above values, preferably 2000-3000Hz. In the present invention, limiting the frequency of the third ultrasonic treatment to a specific range can accelerate the hydroxylation rate and create a uniform hydration layer.
[0069] In some embodiments of the present invention, the plasma treatment process includes sequentially subjecting the cleaned first glass and second glass to glow discharge cleaning, ionized gas bombardment, and neutral gas impact, followed by immersion in water.
[0070] In this invention, plasma surface treatment can physically break bonds and chemically insert them into glass, obtaining E-groups [SiO4] with effects similar to those of acid and alkali treatment. - and D group [SiO3] + Soaking in water and using ultrasound helps the two groups adsorb water molecules to form silanol groups, which then continue to adsorb water molecules to form a hydration layer, thus protecting the reactive groups.
[0071] In some preferred embodiments of the present invention, the glow discharge cleaning time is 2-10 minutes, for example, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, or any value within the range of any two of the above values, preferably 3-5 minutes. In the present invention, if the glow discharge cleaning time is too short, the surface will not be cleaned properly; if the glow discharge cleaning time is too long, it will not be of much help to subsequent processes.
[0072] In some preferred embodiments of the present invention, the vacuum degree of the glow discharge cleaning is 0.1-10 MPa, for example 0.1 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, and any value within any range of any two of the above values, preferably 0.5-3 MPa. In the present invention, if the vacuum degree of the glow discharge cleaning is too low, the cleaning effect will not be achieved; if the vacuum degree of the glow discharge cleaning is too high, it will increase the burden on the equipment and will not be of much help to subsequent processes.
[0073] In some preferred embodiments of the present invention, the bombardment time of the ionized gas is 2-10 min, for example 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, or any value within the range of any two of the above values, preferably 3-6 min. In the present invention, if the bombardment time of the ionized gas is too short, it is not conducive to removing impurities and broken bonds originally adsorbed on the glass surface; if the bombardment time of the ionized gas is too long, it does not help much in removing impurities and broken bonds.
[0074] In some preferred embodiments of the present invention, the neutral gas impact time is 1-10 min, for example 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, and any value within the range of any two of the above values, preferably 4-6 min. In the present invention, if the neutral gas impact time is too short, it is not effective in forming a large number of broken bonds; if the neutral gas impact time is too long, it is not beneficial for further increasing the number of broken bonds.
[0075] In some preferred embodiments of the present invention, the neutral gas is selected from at least one of nitrogen, argon and oxygen.
[0076] In some preferred embodiments of the present invention, the immersion temperature is 25-90°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 70°C, 80°C, 90°C, or any value within any range of two of the above values, preferably 50-60°C. In the present invention, if the immersion temperature is too low, the formation of hydroxyl groups and the hydration layer will be slow; if the immersion temperature is too high, it will be detrimental to safe operation.
[0077] In some preferred embodiments of the present invention, the soaking time is 1-10 min, for example 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, and any value within any range of two of the above values, preferably 3-6 min. In the present invention, if the soaking time is too short, it is difficult to form hydroxyl groups and a hydration layer; if the soaking time is too long, the effect on the formation of reactive groups is not significant.
[0078] In some preferred embodiments of the present invention, the immersion is performed under ultrasonic conditions. The ultrasonic frequency of the ultrasonic conditions is preferably between 1000Hz and 5000Hz, for example, 1000Hz, 1200Hz, 1500Hz, 1800Hz, 2000Hz, 2500Hz, 3000Hz, 3500Hz, 4000Hz, 4500Hz, 5000Hz, and any value within any range of two of the above values, preferably between 2000-3000Hz. In the present invention, limiting the ultrasonic frequency of the ultrasonic conditions to a specific range ensures that bond breaking and hydroxylation occur simultaneously after ion bombardment, while simultaneously forming a hydration layer. Too low a frequency results in a slow formation process, while too high a frequency makes it prone to detachment.
[0079] The method for preparing glass articles with a transition layer according to the present invention is as follows: Figure 1 As shown, material preparation and decorative processing can be carried out according to conventional practices in the field.
[0080] According to a particularly preferred embodiment of the present invention, a method for preparing a glass article with a transition layer is provided, wherein the method comprises: cleaning, surface treating, combining, and heat-treating a first glass and a second glass without pressure to obtain a glass article with a transition layer;
[0081] The assembly process includes bringing the cleaned first and second glass into contact and applying point pressure at 0.1-3 MPa for 20-30 seconds to remove the air layer between the contact surfaces of the first and second glass.
[0082] Before the combination, the flatness of the first glass and the second glass is 0.01-0.03 μm, and the surface roughness is 0.2-0.4 nm;
[0083] The heat treatment includes sequential heating, holding, and cooling; the heating rate is 5-10℃ / min; the holding temperature is 500-650℃; the holding time is 10-30min; and the cooling rate is 8-15℃ / min.
[0084] The surface treatment process includes immersing the cleaned first glass and second glass in a first alkaline treatment solution and performing a first ultrasonic treatment at 45-70°C for 3-5 minutes, and then immersing them in a second alkaline treatment solution and performing a second ultrasonic treatment at 45-70°C for 3-5 minutes; the frequency of the first ultrasonic treatment and the second ultrasonic treatment is 3000-6000Hz.
[0085] The first alkaline treatment solution comprises, by mass percentage: 1-10% sodium hydroxide, 0.1-5% triethanolamine, 0.1-3% sodium carbonate, 0.05-1% sodium dodecylbenzenesulfonate, 0.1-5% fatty alcohol polyoxyethylene ether and 76-97.4% H2O;
[0086] The second alkaline treatment solution is a sodium hydroxide solution with a mass percentage of 1-10%.
[0087] A second aspect of the present invention provides a glass article having a transition layer obtained by the aforementioned preparation method.
[0088] In some embodiments of the present invention, the thickness of the transition layer of the glass article is 0.01-300 μm.
[0089] The transition layer in glass products has a significant impact on the glass's properties. A thicker transition layer results in a more uniform distribution of internal stress. However, an excessively thick transition layer can lead to weak joints in the glass, causing cracks to break off at the weld surface. Therefore, the thickness of the transition layer must be kept appropriate; it should neither be too thin nor too thick.
[0090] A third aspect of the present invention provides a method for observing a transition layer in a glass article, wherein the first glass and the second glass in the glass article are of different colors, and the observation method includes the following steps:
[0091] (1) Grind the glass product at an angle α to expose the entire transition layer;
[0092] (2) Measure the width y of the exposed transition layer;
[0093] (3) The thickness of the transition layer x is calculated by x = y·sinα.
[0094] Since the transition layer cannot be directly observed in colored glass products, the observation method described in this invention involves grinding the colored glass product at a certain angle, then measuring the width of the exposed transition layer, and finally calculating the thickness of the transition layer. The conversion principle for testing the transition layer of colored glass products is as follows: Figure 2 As shown.
[0095] This invention utilizes the different light reflectance and transmittance of two or more different colored glasses, and the different thicknesses of the glass after oblique grinding, to demonstrate the differences in light reflection and refraction, allowing the transition layer to be visually observed.
[0096] In some embodiments of the present invention, the tilt angle α is 1°-89°, such as 1°, 5°, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80°, 85°, 89°, and any value within the range of any two of the above values, preferably 15°-60°.
[0097] In some preferred embodiments of the present invention, the grinding sample is ground under pressure.
[0098] In some preferred embodiments of the present invention, the pressure of the pressurization condition is 0.3-2 MPa, for example 0.3 MPa, 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, and any value within the range of any two of the above values, preferably 0.5-1 MPa.
[0099] In some embodiments of the present invention, the grinding sample includes coarse grinding, fine grinding, and polishing performed sequentially. In the present invention, coarse grinding can improve the reduction of material weight, fine grinding is used to remove the grinding marks left by coarse grinding, and the surface is already relatively smooth after fine grinding. In order to facilitate observation and reduce interference, a polishing step is added. The glass surface obtained by polishing is smooth and easy to observe.
[0100] In some preferred embodiments of the present invention, the coarse grinding time is 60-240s, for example 60s, 100s, 120s, 150s, 200s, 220s, 240s, and any value within the range of any two of the above values, preferably 80-150s.
[0101] In some preferred embodiments of the present invention, the fine grinding time is 60-300s, for example 60s, 100s, 150s, 180s, 200s, 230s, 260s, 300s, and any value within the range of any two of the above values, preferably 100-240s.
[0102] In some preferred embodiments of the present invention, the polishing time is 60-240s, for example 60s, 100s, 120s, 150s, 200s, 220s, 240s, and any value within the range of any two of the above values, preferably 80-150s.
[0103] According to a particularly preferred embodiment of the present invention, a method for observing a transition layer in a glass article, wherein the first glass and the second glass in the glass article are of different colors, the observation method includes the following steps:
[0104] (1) Grind the glass product at an angle α to expose the entire transition layer;
[0105] (2) Measure the width y of the exposed transition layer;
[0106] (3) The thickness of the transition layer x is calculated by x = y·sinα.
[0107] The tilt angle α is 15°-60°; the grinding sample is ground under a pressure of 0.5-1 MPa;
[0108] The grinding sample includes coarse grinding, fine grinding and polishing performed sequentially; the coarse grinding time is 80-150s; the fine grinding time is 100-240s; and the polishing time is 80-150s.
[0109] This invention produces glass products with a distinct transition layer. Compared to existing technologies, the thickness of the transition layer is increased, its distribution is more uniform, and stress concentration is reduced, making it less prone to breakage during subsequent processing. Furthermore, the preparation method described in this invention can shorten the production cycle and greatly improve production efficiency. The observation method for the transition layer in the glass products provided by this invention allows for direct visualization of the transition layer.
[0110] The present invention will be described in detail below through embodiments.
[0111] Unless otherwise specified in the following examples and comparative examples, all conditions were performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments used, unless otherwise specified, are all commercially available products.
[0112] Example 1
[0113] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0114] (1) Clean the 0.7mm thick colorless glass and the 1mm thick colored glass;
[0115] (2) The cleaned colorless glass and colored glass are first immersed in the first alkaline treatment solution for the first ultrasonic treatment, and then immersed in the second alkaline treatment solution for the second ultrasonic treatment.
[0116] The first alkaline treatment solution comprises, by mass percentage: 1% sodium hydroxide, 5% triethanolamine, 3% sodium carbonate, 0.05% sodium dodecylbenzenesulfonate, 0.1% fatty alcohol polyoxyethylene ether and 90.85% H2O;
[0117] The second alkaline treatment solution is a 1% sodium hydroxide solution by mass.
[0118] (3) The colorless glass and colored glass after alkaline treatment are brought into contact and subjected to point pressure treatment so that the air layer between the contact surfaces of the colorless glass and the colored glass is removed and they are combined.
[0119] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0120] The observation method for the glass article with the transition layer includes the following steps:
[0121] (1) Grind the glass product at an angle of 2° at 0.3MPa for 80s, 100s for fine grinding, and 150s for polishing to expose the entire transition layer.
[0122] (2) The width of the exposed transition layer, y = 446.71 μm, was measured using a microscope;
[0123] (3) The thickness of the transition layer x = 15.59 μm was calculated by x = y·sinα.
[0124] Example 2
[0125] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0126] (1) Clean the 0.7mm thick colorless glass and the 1mm thick colored glass;
[0127] (2) The cleaned colorless glass and colored glass are first immersed in the first alkaline treatment solution for the first ultrasonic treatment, and then immersed in the second alkaline treatment solution for the second ultrasonic treatment.
[0128] The first alkaline treatment solution comprises, by mass percentage: 10% sodium hydroxide, 0.1% triethanolamine, 0.1% potassium carbonate, 1% sodium dodecylbenzenesulfonate, 5% fatty alcohol polyoxyethylene ether and 83.8% H2O;
[0129] The second alkaline treatment solution is a 10% sodium hydroxide solution by mass.
[0130] (3) The colorless glass and colored glass after alkaline treatment are brought into contact and subjected to point pressure treatment so that the air layer between the contact surfaces of the colorless glass and the colored glass is removed and they are combined.
[0131] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0132] The observation method for the glass article with the transition layer includes the following steps:
[0133] (1) The glass product is rough-grinded at an angle of 81° and at 2MPa for 150s, fine-grinded for 240s, and polished for 80s to expose the entire transition layer.
[0134] (2) The width of the exposed transition layer, y = 15.25 μm, was measured using a microscope;
[0135] (3) The thickness of the transition layer is calculated to be x = 15.06 μm by using x = y·sinα.
[0136] Example 3
[0137] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0138] (1) Clean the 0.5mm thick colorless glass and the 0.8mm thick colored glass;
[0139] (2) The cleaned colorless glass and the second glass are first immersed in the first alkaline treatment solution for the first ultrasonic treatment, and then immersed in the second alkaline treatment solution for the second ultrasonic treatment.
[0140] The first alkaline treatment solution comprises, by mass percentage: 3% potassium hydroxide, 1% triethanolamine, 0.2% potassium carbonate, 0.08% sodium dodecylbenzenesulfonate, 0.2% fatty alcohol polyoxyethylene ether, and 95.52% H2O;
[0141] The second alkaline treatment solution is a 3% potassium hydroxide solution by mass.
[0142] (3) The colorless glass and colored glass after alkaline treatment are brought into contact and subjected to point pressure treatment so that the air layer between the contact surfaces of the colorless glass and the colored glass is removed and they are combined.
[0143] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0144] The observation method for the glass article with the transition layer includes the following steps:
[0145] (1) Grind the glass product at an angle of 15° at 1MPa for 100s, 200s for fine grinding, and 120s for polishing to make the transition layer visible to the naked eye.
[0146] (2) The width of the exposed transition layer was measured to be y = 56.37 μm using a microscope;
[0147] (3) The thickness of the transition layer x = 14.59 μm was calculated by x = y·sinα.
[0148] Finished product image as shown Figure 3As shown. The grinding sample diagram is as follows. Figure 4a As shown, the micrograph is as follows Figure 4b As shown in the photograph, the presence of the transition layer is clearly visible, and microscopic observation is also very clear.
[0149] Example 4
[0150] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0151] (1) Clean the 0.5mm thick colorless glass and the 0.8mm thick colored glass;
[0152] (2) The cleaned colorless glass and the second glass are first immersed in the first alkaline treatment solution for the first ultrasonic treatment, and then immersed in the second alkaline treatment solution for the second ultrasonic treatment.
[0153] The first alkaline treatment solution comprises, by mass percentage: 8% potassium hydroxide, 1% triethanolamine, 0.2% potassium carbonate, 0.07% sodium dodecylbenzenesulfonate, 2% fatty alcohol polyoxyethylene ether, and 88.73% H2O.
[0154] The second alkaline treatment solution is a 5% potassium hydroxide solution by mass.
[0155] (3) The colorless glass and colored glass after alkaline treatment are brought into contact and subjected to point pressure treatment so that the air layer between the contact surfaces of the colorless glass and the colored glass is removed and they are combined.
[0156] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0157] The observation method for the glass article with the transition layer includes the following steps:
[0158] (1) The glass product is subjected to rough grinding for 60s, fine grinding for 300s, and polishing for 240s at an inclination angle of 60° and 0.5MPa, so that the transition layer is visible to the naked eye;
[0159] (2) The width of the exposed transition layer was measured to be y = 16.4 μm using a microscope;
[0160] (3) The thickness of the transition layer x = 14.2 μm was calculated by x = y·sinα.
[0161] Example 5
[0162] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0163] (1) Clean the 0.5mm thick colorless glass and the 0.8mm thick colored glass;
[0164] (2) The cleaned colorless glass and the second glass are first immersed in the first alkaline treatment solution for the first ultrasonic treatment, and then immersed in the second alkaline treatment solution for the second ultrasonic treatment.
[0165] The first alkaline treatment solution comprises, by mass percentage: 8% potassium hydroxide, 1% triethanolamine, 0.2% potassium carbonate, 0.07% sodium dodecylbenzenesulfonate, 2% fatty alcohol polyoxyethylene ether, and 88.73% H2O.
[0166] The second alkaline treatment solution is a 5% potassium hydroxide solution by mass.
[0167] (3) The colorless glass and colored glass after alkaline treatment are brought into contact and subjected to point pressure treatment so that the air layer between the contact surfaces of the colorless glass and the colored glass is removed and they are combined.
[0168] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0169] The observation method for the glass article with the transition layer includes the following steps:
[0170] (1) The glass product is subjected to rough grinding for 240s, fine grinding for 60s, and polishing for 60s at an inclination angle of 50° and 1.65MPa, so that the transition layer is visible to the naked eye.
[0171] (2) The width of the exposed transition layer was measured to be y = 18.62 μm using a microscope;
[0172] (3) The thickness of the transition layer x = 14.26 μm was calculated by x = y·sinα.
[0173] Example 6
[0174] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0175] (1) Clean the 0.7mm thick colorless glass and the 1mm thick colorless glass;
[0176] (2) The cleaned colorless glass and colorless glass are first immersed in the first acidic treatment solution for the third ultrasonic treatment, and then immersed in the second acidic treatment solution for the fourth ultrasonic treatment.
[0177] The first acidic treatment solution comprises, by mass percentage: 1% HF, 10% H3PO4, 0.5% HNO3 and 88.5% H2O;
[0178] The second acidic treatment solution is a 1% hydrochloric acid solution by mass.
[0179] (3) Make the acid-treated colorless glass and colorless glass come into contact and perform point pressure treatment to remove the air layer between the colorless glass and colorless glass contact surfaces and then combine them.
[0180] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0181] Example 7
[0182] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0183] (1) Clean the 0.8mm thick colorless glass and the 1.2mm thick colorless glass;
[0184] (2) The cleaned colorless glass and colorless glass are first immersed in the first acidic treatment solution for the third ultrasonic treatment, and then immersed in the second acidic treatment solution for the fourth ultrasonic treatment.
[0185] The first acidic treatment solution comprises, by mass percentage: 5% HF, 1% H3PO4, 10% HNO3 and 84% H2O;
[0186] The second acidic treatment solution is a 10% hydrochloric acid solution by mass.
[0187] (3) Make the acid-treated colorless glass and colorless glass come into contact and perform point pressure treatment to remove the air layer between the colorless glass and colorless glass contact surfaces and then combine them.
[0188] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0189] Example 8
[0190] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0191] (1) Clean the 0.7mm thick colorless glass and the 1.2mm thick colorless glass;
[0192] (2) After cleaning, the colorless glass and the colorless glass are subjected to glow discharge cleaning, ionized gas bombardment and nitrogen impact in sequence, and then soaked in water under ultrasonic conditions.
[0193] (3) The plasma-treated colorless glass and colorless glass are brought into contact and subjected to point pressure treatment to remove the air layer between the contact surfaces of the colorless glass and colorless glass and then combine them.
[0194] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0195] Example 9
[0196] According to the operating parameters in Table 1, a method for preparing a glass article with a transition layer includes the following steps:
[0197] (1) Clean the 0.7mm thick colorless glass and the 1mm thick colorless glass;
[0198] (2) After cleaning, the colorless glass and the colorless glass are successively subjected to glow discharge cleaning, ionized gas bombardment, and argon gas impact, and then soaked in water under ultrasonic conditions.
[0199] (3) The plasma-treated colorless glass and colorless glass are brought into contact and subjected to point pressure treatment to remove the air layer between the contact surfaces of the colorless glass and colorless glass and then combine them.
[0200] (4) The assembled glass is heated, kept heated and cooled in sequence without pressure to obtain a glass product with a transition layer.
[0201] Table 1
[0202]
[0203]
[0204]
[0205] Note: "-" in Table 1 indicates that the operation is not performed.
[0206] Comparative Example 1
[0207] Glass articles are prepared using the preparation method disclosed in CN110790517A.
[0208] Comparative Example 2
[0209] Glass articles with transition layers were prepared according to the method in Example 3, except that the combination method was different.
[0210] (3) Make the colorless glass and colored glass after alkaline treatment come into contact in the solution to remove the air layer.
[0211] Comparative Example 3
[0212] A glass article with a transition layer is prepared according to the method of Example 3, with the difference that:
[0213] (4) The combined glass is subjected to sequential heating, heat preservation, and cooling under a pressurized condition of 0.2 MPa to obtain the glass article with a transition layer.
[0214] Test Example 1
[0215] A cross-sectional micrograph of the sample is obtained through a microscope.
[0216] Using a purchased 7-inch domestic screen / OLED screen polarizer, place the 0° horizontal line of the vertical screen on one side of the glass, place the 90° vertical line of the vertical screen perpendicular to it on the other side of the glass, ensuring that the horizontal line of the vertical screen is perpendicular to the vertical line of the vertical screen. Observe against a light source to check the stress condition: a bright area will appear on the stress-containing film, while there is no change on the film without stress, thereby obtaining the polarizer schematic diagram of the stress distribution of the sample.
[0217] The cross-sectional micrograph of the sample of the glass article obtained in Example 3 is shown in Figure 5a , and the polarizer schematic diagram of the stress distribution of the sample is shown in Figure 5b .
[0218] The cross-sectional micrograph of the sample of the glass article obtained in Comparative Example 1 is shown in Figure 6a , and the polarizer schematic diagram of the stress distribution of the sample is shown in Figure 6b .
[0219] It can be seen from the micrographs that there is a significant difference between the products obtained in Example 3 and Comparative Example 1. The glass article in Comparative Example 1 has no obvious transition layer after direct fracture, and the polarizer schematic diagram of stress distribution shows that the stress is mainly concentrated at the four corners, that is, the four corners are the most prone to fracture; the glass article in Example 3 has an obvious transition layer after direct fracture, and there is also stress concentration at the four corners after pressurization, but it is much less prominent than the former. This indicates that the presence of the transition layer helps to reduce stress concentration.
[0220] Test Example 2
[0221] The ball drop test is carried out with reference to GB / T 39814-2021 "Test Method for Impact Strength of Ultra-thin Glass - Ball Drop Method".
[0222] The 4PB test is carried out with reference to GB / T 37781-2019 "Test Method for Bending Strength of Glass Materials".
[0223] The thrust test follows the customer's standard, which generally requires that the glass does not fracture under a thrust of 100N, that is, greater than 8.34 MPa. The test method is to cut the integrated glass into a size of 8mm×1.5mm, use the thrust method to test the bonding force, and the pressing speed of the thrust test is 5 mm / min.
[0224] The results are shown in Table 2.
[0225] Table 2
[0226] serial number Ball drop test (mm) 4PB test (MPa) Thrust test (MPa) Example 1 55 776.8 29.32 Example 2 55 773.6 30.15 Example 3 45 605.3 20.18 Example 4 45 600.8 19.93 Example 5 45 601.2 20.12 Example 6 50 649.7 23.52 Comparative Example 1 40 603.9 22.61 Comparative Example 2 35 573.3 16.17 Comparative Example 3 40 602.5 21.73
[0227] As can be seen from the results in Table 2, the embodiment using the solution-free, point-press combined, non-pressurized, and heat-treated integrated process of the present invention has better impact resistance and bending resistance. Compared with Comparative Examples 1, 2, and 3, Example 3 has better drop ball test results, and the values of the 4PB test and thrust test are close. This indicates that the integrated glass with a clear transition layer has better impact resistance. Moreover, the elimination of pressurization shortens the production time, reduces production energy consumption, and improves production efficiency, resulting in significantly better performance.
[0228] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing a glass article with a transition layer, characterized in that, The preparation method includes: cleaning, surface treating, combining, and heat-treating the first glass and the second glass without pressure to obtain a glass product with a transition layer; The assembly process includes bringing the cleaned first glass and second glass into contact and applying point pressure to remove the air layer between the contact surfaces of the first glass and the second glass. The pressure of the point pressurization process is 0.05-5 MPa; The surface treatment is an alkaline solution treatment; The alkaline treatment process includes immersing the cleaned first glass and second glass in a first alkaline treatment solution for a first ultrasonic treatment, and then immersing them in a second alkaline treatment solution for a second ultrasonic treatment. The first alkaline treatment solution, by mass percentage, comprises: 1-10% alkali, 0.1-5% triethanolamine, 0.1-3% alkaline salt, 0.05-1% sodium dodecylbenzenesulfonate, 0.1-5% fatty alcohol polyoxyethylene ether, and 76-97.4% H2O. The alkaline treatment forms a hydration layer; during the heat treatment process, the hydration layer transforms into a transition layer. The heat treatment includes sequential heating, holding, and cooling; the holding temperature is 300-700℃.
2. The preparation method according to claim 1, wherein, The pressure for the point pressurization process is 0.1-3 MPa.
3. The preparation method according to claim 1, wherein, The time for the point pressurization process is 5-60 seconds; And / or, before the combination, the flatness of the first glass and the second glass is 0.001-0.05 μm; And / or, prior to the combination, the surface roughness of the first glass and the second glass is 0.01-1 nm.
4. The preparation method according to claim 3, wherein, The time for the point pressurization process is 20-30 seconds; And / or, before the combination, the flatness of the first glass and the second glass is 0.01-0.03 μm; And / or, prior to the combination, the surface roughness of the first and second glass is 0.2-0.4 nm.
5. The preparation method according to claim 1, wherein, The heating rate is 0.5-20℃ / min; And / or, the heat preservation time is 1-60 min; And / or, the cooling rate is 1-30°C / min.
6. The preparation method according to claim 5, wherein, The heating rate is 5-10℃ / min; And / or, the insulation temperature is 500-650℃; And / or, the heat preservation time is 10-30 minutes; And / or, the cooling rate is 8-15°C / min.
7. The preparation method according to any one of claims 1-6, wherein, The alkali is sodium hydroxide and / or potassium hydroxide; And / or, the alkaline salt is sodium carbonate and / or potassium carbonate; And / or, the temperature of the first ultrasonic treatment is 25-90°C; And / or, the duration of the first ultrasonic treatment is 1-10 min; And / or, the frequency of the first ultrasonic treatment is 1000-8000Hz; And / or, the second alkaline treatment solution is an alkaline solution with a mass percentage of 1-10%; And / or, the temperature of the second ultrasonic treatment is 25-90°C; And / or, the duration of the second ultrasonic treatment is 1-10 min; And / or, the frequency of the second ultrasonic treatment is 1000-8000Hz.
8. The preparation method according to claim 7, wherein, The temperature of the first ultrasonic treatment is 45-70℃; And / or, the duration of the first ultrasonic treatment is 3-5 minutes; And / or, the frequency of the first ultrasonic treatment is 3000-6000Hz; And / or, the base in the alkaline solution is sodium hydroxide and / or potassium hydroxide; And / or, the temperature of the second ultrasonic treatment is 45-70°C; And / or, the duration of the second ultrasonic treatment is 3-5 minutes; And / or, the frequency of the second ultrasonic treatment is 3000-6000Hz.
9. A glass article having a transition layer obtained by the preparation method according to any one of claims 1-8.
10. The glass article according to claim 9, wherein, The thickness of the transition layer in the glass product is 0.01-300 μm.
Citation Information
Patent Citations
Shell and preparation method thereof, display device and terminal equipment
CN110790517A
Glass bonding method
CN113415981A