A composite PE plastic and its preparation process

By using functional compatibilizers and modified clay mineral fillers in polyethylene plastics, the flame retardant and mechanical properties of polyethylene plastics are improved, and the problems of poor flame retardant and poor mechanical properties of polyethylene plastics are solved. A composite material with high strength and high flame retardant is achieved.

CN117820746BActive Publication Date: 2024-12-03GUIZHOU BOYU NEW ENERGY TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311793725.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-03
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

Polyethylene plastics have poor flame retardant properties and poor mechanical properties, which limit their application in industries with high strength and high flame retardant requirements.

Method used

Low-density polyethylene containing silicon-phosphorus synergistic flame retardant elements and epoxy groups in the structure are used as functional compatibility agents, and illite modified with surface branched polyethyleneimine is used as a modified clay mineral filler. Blending and high-temperature granulation technology improves the flame retardant and mechanical properties of polyethylene plastics.

Benefits of technology

The flame retardant and mechanical properties of composite polyethylene plastics are significantly improved, with an ultimate oxygen index of 33.4%. By improving the compatibility between polyethylene and filler, the long-term flame retardant effect and mechanical properties of the material are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117820746B_ABST
    Figure CN117820746B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of plastics, and discloses a composite PE plastic and a preparation process thereof. The composite PE plastic is prepared by using high-density polyethylene, a functional compatibilizer, a modified clay mineral filler, a lubricant, an antioxidant and a pigment filler as raw materials and adopting a blending-granulation process, wherein the functional compatibilizer is a low-density polyethylene containing silicon-phosphorus synergistic flame retardant elements and epoxy groups in the structure, and the modified clay mineral filler is illite with branched polyethyleneimine grafted on the surface. The synergistic effect of the functional compatibilizer and the modified clay mineral filler can effectively improve the problem of poor flame retardant performance of polyethylene plastic products, so that the prepared composite polyethylene plastic has good flame retardant performance and mechanical properties, and its application range can be effectively broadened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, and in particular to a composite PE plastic and a preparation process thereof. Background Art

[0002] Polyethylene, referred to as PE, is a thermoplastic resin that is non-toxic, odorless, chemically stable, and has excellent electrical insulation properties. It currently occupies an important position in industries such as pipes, packaging materials, building materials, and wires and cables. However, due to its own structure, polyethylene has extremely poor flame retardancy, with a limiting oxygen index of approximately 17.4, making it a flammable material. Therefore, polyethylene plastic products generally have the disadvantage of poor flame resistance. In addition, polyethylene will produce smoke while burning, accompanied by molten dripping behavior, which not only damages the environment, but also causes the scope of combustion to expand, the fire to develop rapidly, and thus causes serious consequences. This has led to the gradual restriction of the development of polyethylene plastic products in industries such as cables that have high flame retardancy requirements. In addition, the mechanical properties of polyethylene are also relatively general, and are gradually unable to meet the demand for high-strength plastic products. Therefore, there is an urgent need to improve polyethylene plastic products.

[0003] In the prior art, a blending modification method is often used to enhance and modify polyethylene plastic products. For example, the invention patent with application number CN202310011341.8 discloses a high-performance flame-retardant polyethylene sheath material and a preparation method thereof. The components include layered silicates, mesoporous silica, wollastonite fibers, powdered PN series flame retardants and liquid phosphate flame retardants. Loaded flame retardant carbon-forming agents can effectively improve the mechanical properties and flame retardancy of the resulting flame-retardant polyethylene material. However, due to the non-polarity of the polyethylene molecular structure, the compatibility between polyethylene and most polar polymers and inorganic fillers is poor, which in turn has a negative impact on the mechanical properties of polyethylene. Therefore, if this modification method is to be used, the compatibility problem between the additive and the polyethylene matrix must be solved first to ensure that the obtained polyethylene plastic product can achieve the ideal modification effect. Summary of the invention

[0004] The purpose of the present invention is to provide a composite PE plastic and a preparation process thereof, which solves the problems of poor flame retardancy and poor mechanical properties of polyethylene plastic.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A composite PE plastic, comprising the following raw materials by weight: 95-100 parts of high-density polyethylene, 5-10 parts of functional compatibilizer, 2-5.5 parts of modified clay mineral filler, 1-3 parts of lubricant, 0.5-1 parts of antioxidant, and 10-20 parts of pigment filler;

[0007] The functional compatibilizer is a low-density polyethylene containing silicon-phosphorus synergistic flame retardant elements and epoxy groups in its structure;

[0008] The modified clay mineral filler is illite with branched polyethyleneimine grafted on the surface.

[0009] Furthermore, the lubricant is any one of paraffin, polyethylene wax, calcium stearate, zinc stearate or stearic acid; the antioxidant is any one of antioxidant 1010, antioxidant 1098 or antioxidant DLTP; the color filler is any one of carbon black or titanium dioxide.

[0010] Furthermore, the preparation method of the functional compatibilizer comprises the following steps:

[0011] Step A: low-density polyethylene, (4-vinylphenyl) dimethylsilane, glycidyl methacrylate and benzoyl peroxide are stirred and mixed uniformly, and then added into a torque rheometer, melt-grafted at a temperature of 180-190° C. for 5-10 minutes, and then cooled and discharged to obtain a low-density polyethylene intermediate material;

[0012] Step B: Add low-density polyethylene intermediate material to xylene, turn on the heating until the temperature reaches 80-90°C, stir until completely dissolved, add 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide and catalyst, after the addition, pass nitrogen, continue stirring for 4-8 hours, cool and discharge the material to obtain a functional compatibilizer.

[0013] Furthermore, in step A, the mass ratio of the low-density polyethylene, (4-vinylphenyl)dimethylsilane, glycidyl methacrylate and benzoyl peroxide is 10:1-2:1.2-2.5:0.05-0.1.

[0014] Furthermore, in step A, the catalyst is trifluoroacetic acid.

[0015] In the above technical scheme, benzoyl peroxide is used as an initiator to initiate the in-situ polymerization of (4-vinylphenyl) dimethylsilane and glycidyl methacrylate in the low-density polyethylene molecular chain to form a low-density polyethylene intermediate material containing epoxy groups and Si-H bonds in the structure. Under the catalytic action of trifluoroacetic acid, the Si-H bonds can react with the active hydroxyl groups in the 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide structure, thereby introducing a silicon-phosphorus synergistic flame retardant into the low-density polyethylene molecular chain to obtain a functional compatibilizer.

[0016] Furthermore, the preparation method of the modified clay mineral filler comprises the following steps:

[0017] Step A1: After the acidified illite is mixed with toluene to form a uniform dispersion, chlorine-substituted isocyanate and dibutyltin dilaurate are added to the dispersion. After the addition, stirring and heating are started until the system temperature reaches 70-80° C., and after keeping the temperature for 6-12 hours, the solid material is separated to obtain halogenated illite;

[0018] Step A2: Mix the halogenated illite and 1,4-dioxane, disperse them uniformly by ultrasonication, add branched polyethyleneimine and triethylamine and stir evenly, raise the temperature to 50-60°C, stir at a constant temperature for 4-6 hours, centrifuge the solid product, wash and vacuum dry it, and obtain a modified clay mineral filler.

[0019] Furthermore, in step A1, the acidification process of the illite is specifically as follows: the illite powder is put into a hydrochloric acid solution with a mass fraction of 1-5%, stirred and mixed, heated to 60-65°C, stirred at a constant temperature for 1-3 hours, the solid material is separated, washed with deionized water until neutral, and vacuum dried.

[0020] Furthermore, in step A1, the chlorine-substituted isocyanate is any one of chloroethyl isocyanate or 3-chloropropyl isocyanate.

[0021] Furthermore, in step A1, the average molecular weight of the branched polyethyleneimine is 10,000.

[0022] In the above technical scheme, after the illite is treated with acid, Si-OH can be generated on the surface. Dibutyltin dilaurate is used as a catalyst to catalyze the reaction of the isocyanate group of the chlorine-substituted isocyanate with Si-OH, and the halogen group is modified on the surface of the illite to obtain halogenated illite, which can further react with the amino group in the branched polyethyleneimine structure under the action of triethylamine, thereby modifying the branched polyethyleneimine on the surface of the illite to obtain a modified clay mineral filler.

[0023] A preparation process of composite PE plastics comprises the following steps:

[0024] Step 1: Weigh each raw material by weight and set aside;

[0025] Step 2: Pour high-density polyethylene, functional compatibilizer, modified clay mineral filler, lubricant, antioxidant, and pigment filler into a mixer, control the temperature in the mixer to 90-100° C., and stir and mix at a stirring speed of 300-500 r / min for 20-40 minutes to form a premix;

[0026] Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170±5℃, Zone 2 175±5℃, Zone 3 185±5℃, Zone 4 195±5℃, Zone 5 200±5℃, Zone 6 205±5℃, Zone 7 200±5℃, Zone 8 180±5℃, Zone 9 170±5℃, and the die temperature is 165±5℃. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0027] Beneficial effects of the present invention:

[0028] 1) The present invention prepares a low-density polyethylene containing a silicon-phosphorus synergistic flame retardant and an epoxy group in its structure as a functional compatibilizer, and blends it with a high-density polyethylene. The synergistic flame retardant effect of the silicon-phosphorus flame retardant is utilized to enable the prepared composite polyethylene plastic to exhibit excellent flame retardant properties. Tests show that the limiting oxygen index of the composite polyethylene plastic prepared by the present invention can reach 33.4%, and because the flame retardant exists in the composite polyethylene plastic in the form of a chemical bond connection, the migration and volatilization of the flame retardant can be avoided, thereby achieving a long-term flame retardant modification effect.

[0029] 2) The present invention prepares illite with surface modification of branched polyethyleneimine as filler. During the blending and high-temperature granulation process, active groups such as primary amine and secondary amine in the branched polyethyleneimine structure can interact with epoxy groups in the functional compatibilizer structure to form mutual connections, thereby effectively improving the compatibility between the illite and the polyethylene matrix. Therefore, the illite can be evenly arranged in the composite polyethylene plastic, and play a physical barrier role when the composite polyethylene plastic burns. In addition, the non-combustible gas generated by the nitrogen element in the branched polyethyleneimine during combustion can also effectively reduce the oxygen concentration, form an oxygen-free environment, and prevent continuous combustion, thereby further improving the flame retardant properties of the composite polyethylene plastic.

[0030] 3) The branched polyethyleneimine structure contained in the modified clay mineral filler prepared by the present invention can penetrate and entangle with the polyethylene molecular chain to form a bridging-crack anchoring stable structure, so that the mechanical properties of the composite polyethylene plastic are effectively enhanced, which is conducive to broadening the application range of the composite polyethylene plastic.

[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0033] Figure 1 The infrared test spectra of the functional compatibilizers in the embodiments and comparative examples of the present invention;

[0034] Figure 2 It is the infrared test spectrum of the modified clay mineral filler in the examples and comparative examples of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] A composite PE plastic, comprising the following raw materials by weight: 95 parts of high-density polyethylene, 5 parts of functional compatibilizer, 2 parts of modified clay mineral filler, 1 part of lubricant paraffin, 0.5 parts of antioxidant 1010, and 10 parts of color filler titanium dioxide;

[0038] The preparation method of the composite PE plastic comprises the following steps:

[0039] Step 1: Weigh each raw material by weight and set aside;

[0040] Step 2: Pour high-density polyethylene, functional compatibilizer, modified clay mineral filler, lubricant paraffin, antioxidant 1010, and pigment filler titanium dioxide into a mixer, control the temperature in the mixer to 90° C., and stir and mix at a stirring speed of 300 r / min for 40 minutes to form a premix;

[0041] Step 3: Place the premix in the extruder, set the temperatures of each zone of the extruder as follows: Zone 1 165°C, Zone 2 170°C, Zone 3 180°C, Zone 4 190°C, Zone 5 195°C, Zone 6 200°C, Zone 7 195°C, Zone 8 175°C, Zone 9 165°C, and the die temperature is 160°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0042] Example 2

[0043] A composite PE plastic, comprising the following raw materials by weight: 98 parts of high-density polyethylene, 8 parts of functional compatibilizer, 5 parts of modified clay mineral filler, 2 parts of lubricant polyethylene wax, 0.8 parts of antioxidant 1098, and 15 parts of color filler titanium dioxide;

[0044] The preparation method of the composite PE plastic comprises the following steps:

[0045] Step 1: Weigh each raw material by weight and set aside;

[0046] Step 2: Pour high-density polyethylene, functional compatibilizer, modified clay mineral filler, lubricant polyethylene wax, antioxidant 1098, and pigment filler titanium dioxide into a mixer, control the temperature in the mixer to 95° C., and stir and mix at a stirring speed of 400 r / min for 30 minutes to form a premix;

[0047] Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170°C, Zone 2 175°C, Zone 3 185°C, Zone 4 195°C, Zone 5 200°C, Zone 6 205°C, Zone 7 200°C, Zone 8 180°C, Zone 9 170°C, and the die temperature is 165°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0048] Example 3

[0049] A composite PE plastic, comprising the following raw materials by weight: 100 parts of high-density polyethylene, 10 parts of functional compatibilizer, 5.5 parts of modified clay mineral filler, 3 parts of lubricant stearic acid, 1 part of antioxidant DLTP, and 20 parts of color filler titanium dioxide;

[0050] The preparation method of the composite PE plastic comprises the following steps:

[0051] Step 1: Weigh each raw material by weight and set aside;

[0052] Step 2: Pour high-density polyethylene, functional compatibilizer, modified clay mineral filler, lubricant stearic acid, antioxidant DLTP, and pigment filler titanium dioxide into a mixer, control the temperature in the mixer to 100° C., and stir and mix at a stirring speed of 500 r / min for 20 minutes to form a premix;

[0053] Step 3: Place the premix in the extruder, set the temperatures of each zone of the extruder as follows: Zone 1 175°C, Zone 2 180°C, Zone 3 190°C, Zone 4 200°C, Zone 5 205°C, Zone 6 210°C, Zone 7 205°C, Zone 8 185°C, Zone 9 175°C, and the die head temperature is 170°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0054] Comparative Example 1

[0055] A composite PE plastic, comprising the following raw materials by weight: 98 parts of high-density polyethylene, 8 parts of maleic anhydride grafted polyethylene, 5 parts of modified clay mineral filler, 2 parts of lubricant polyethylene wax, 0.8 parts of antioxidant 1098, and 15 parts of color filler titanium dioxide;

[0056] The preparation method of the composite PE plastic comprises the following steps:

[0057] Step 1: Weigh each raw material by weight and set aside;

[0058] Step 2: Pour high-density polyethylene, maleic anhydride grafted polyethylene, modified clay mineral filler, lubricant polyethylene wax, antioxidant 1098, and pigment filler titanium dioxide into a mixer, control the temperature in the mixer to 95° C., and stir and mix at a stirring speed of 400 r / min for 30 minutes to form a premix;

[0059] Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170°C, Zone 2 175°C, Zone 3 185°C, Zone 4 195°C, Zone 5 200°C, Zone 6 205°C, Zone 7 200°C, Zone 8 180°C, Zone 9 170°C, and the die temperature is 165°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0060] The maleic anhydride grafted polyethylene was purchased from Dongguan Taotao Plastic Raw Materials Co., Ltd.

[0061] Comparative Example 2

[0062] A composite PE plastic, comprising the following raw materials by weight: 98 parts of high-density polyethylene, 8 parts of functional compatibilizer, 5 parts of illite, 2 parts of lubricant polyethylene wax, 0.8 parts of antioxidant 1098, and 15 parts of color filler titanium dioxide;

[0063] The preparation method of the composite PE plastic comprises the following steps:

[0064] Step 1: Weigh each raw material by weight and set aside;

[0065] Step 2: Pour high-density polyethylene, functional compatibilizer, illite, lubricant polyethylene wax, antioxidant 1098, and pigment filler titanium dioxide into a mixer, control the temperature in the mixer to 95° C., and stir and mix at a stirring speed of 400 r / min for 30 minutes to form a premix;

[0066] Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170°C, Zone 2 175°C, Zone 3 185°C, Zone 4 195°C, Zone 5 200°C, Zone 6 205°C, Zone 7 200°C, Zone 8 180°C, Zone 9 170°C, and the die temperature is 165°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0067] Comparative Example 3

[0068] A composite PE plastic, comprising the following raw materials by weight: 98 parts of high-density polyethylene, 8 parts of functional compatibilizer, 2 parts of lubricant polyethylene wax, 0.8 parts of antioxidant 1098, and 15 parts of color filler titanium dioxide;

[0069] The preparation method of the composite PE plastic comprises the following steps:

[0070] Step 1: Weigh each raw material by weight and set aside;

[0071] Step 2: Pour high-density polyethylene, functional compatibilizer, lubricant polyethylene wax, antioxidant 1098, and pigment titanium dioxide into a mixer, control the temperature in the mixer to 95°C, and stir and mix at a stirring speed of 400 r / min for 30 minutes to form a premix;

[0072] Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170°C, Zone 2 175°C, Zone 3 185°C, Zone 4 195°C, Zone 5 200°C, Zone 6 205°C, Zone 7 200°C, Zone 8 180°C, Zone 9 170°C, and the die temperature is 165°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0073] Comparative Example 4

[0074] A composite PE plastic, comprising the following raw materials by weight: 98 parts of high-density polyethylene, 8 parts of maleic anhydride grafted polyethylene, 2 parts of lubricant polyethylene wax, 10980.8 parts of antioxidant, and 15 parts of color filler titanium dioxide;

[0075] The preparation method of the composite PE plastic comprises the following steps:

[0076] Step 1: Weigh each raw material by weight and set aside;

[0077] Step 2: Pour high-density polyethylene, maleic anhydride grafted polyethylene, lubricant polyethylene wax, antioxidant 1098, and pigment filler titanium dioxide into a mixer, control the temperature in the mixer to 95° C., and stir and mix at a stirring speed of 400 r / min for 30 minutes to form a premix;

[0078] Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170°C, Zone 2 175°C, Zone 3 185°C, Zone 4 195°C, Zone 5 200°C, Zone 6 205°C, Zone 7 200°C, Zone 8 180°C, Zone 9 170°C, and the die temperature is 165°C. After the melt extrusion granulation process, the composite PE plastic can be obtained.

[0079] The functional compatibilizer used in the above examples and comparative examples is prepared by the following steps:

[0080] Step A: 20 g of low-density polyethylene, 3.5 g of (4-vinylphenyl) dimethylsilane, 4 g of glycidyl methacrylate and 0.1 g of benzoyl peroxide were stirred and mixed uniformly, and then added into a torque rheometer, melt-grafted at 185° C. for 5 min, and then cooled and discharged to obtain a low-density polyethylene intermediate material;

[0081] Step B: Add 5 g of low-density polyethylene intermediate material to xylene, turn on the heating to 85°C, stir until completely dissolved, add 1 g of 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide and 0.2 g of trifluoroacetic acid, after the addition, pass nitrogen, continue stirring for 6 hours, cool and discharge the material to obtain a functional compatibilizer.

[0082] Take the functional compatibilizer sample, make it into potassium bromide tablets, and perform infrared characterization on it. The results are shown in Figure 1 , analysis shows that 3000~3100cm -1 It is the characteristic absorption peak of CH in benzene ring; 2870~2945cm -1 It is the characteristic absorption peak of CH in methyl and methylene; 1748cm -1 It is the characteristic absorption peak of C=O in glycidyl methacrylate; 1267cm -1 It is the characteristic absorption peak of O=P; 1081cm -1 It is the characteristic absorption peak of Si-O; 901cm -1 The sum is 843cm -1 It is the characteristic absorption peak of epoxy group.

[0083] The modified clay mineral fillers used in the above examples and comparative examples are prepared by the following steps:

[0084] Step A1: 4 g of illite powder with an average particle size of 1 μm is added to 180 mL of a 2% hydrochloric acid solution, stirred and mixed, and then heated to 60° C. After constant temperature stirring for 2 h, the solid material is separated, washed with deionized water until neutral, and vacuum dried to obtain acidified illite;

[0085] Step A2: 3.5 g of the acidified illite was mixed with toluene to form a uniform dispersion, and 2.8 g of chloroethyl isocyanate and 0.1 g of dibutyltin dilaurate were added to the dispersion. After the addition, stirring and heating were started until the system temperature reached 75° C. After keeping the temperature for 9 hours, the solid material was separated to obtain halogenated illite;

[0086] Step A3: 2 g of halogenated illite was mixed with 1,4-dioxane, and ultrasonically dispersed uniformly. Then, 1.2 g of branched polyethyleneimine with an average molecular weight of 10,000 and 0.8 g of triethylamine were added and stirred evenly. The temperature was raised to 60° C., and after constant temperature stirring for 4 hours, the solid product was centrifuged out, and the modified clay mineral filler was obtained after washing and vacuum drying.

[0087] Figure 2 This is the infrared test spectrum of the modified clay mineral filler. The analysis shows that 3398-3455cm -1 NH stretching vibration peak; 2850~2930cm -1 The CH stretching vibration peaks of methylene and methyl groups; 1749 cm -1 Ester group C=O stretching vibration peak; 1055~1120cm -1 It is the characteristic absorption peak of Si-O.

[0088] Performance Testing

[0089] Refer to the national standard GB / T 1040.2-2022, test the tensile properties, and set the tensile rate to 100mm / min;

[0090] Refer to the national standard GB / T 9341-2008 to test the bending performance;

[0091] Refer to the national standard GB / T 14152-2001 to test the impact performance;

[0092] Refer to the national standard GB / T 2406.2-2009, test the limiting oxygen index, and the test results are recorded in the following table:

[0093] Tensile strength / MPa Bending strength / MPa <![CDATA[Impact strength / kJ / m 2 > Oxygen index / % Example 1 46.7 62.8 71.6 32.9 Example 2 47.5 63.2 72.1 33.4 Example 3 47.0 63.1 71.9 33.1 Comparative Example 1 45.5 60.6 67.3 25.8 Comparative Example 2 41.3 50.9 56.0 31.0 Comparative Example 3 33.2 46.5 49.8 28.6 Comparative Example 4 31.9 44.1 46.5 18.3

[0094] It can be observed from the test data that the composite PE plastics prepared in Examples 1 to 3 of the present invention have good flame retardant properties and excellent mechanical properties. In Comparative Example 1, maleic anhydride grafted polyethylene is used as a compatibilizer, resulting in the prepared composite PE plastic not containing silicon-phosphorus synergistic flame retardant, so the flame retardant properties are significantly reduced. In Comparative Example 2, illite without surface modification is used as a filler, which may be partially agglomerated, so compared with the embodiments, the mechanical properties and flame retardant properties are reduced to varying degrees. In Comparative Example 3, no clay mineral filler is added, so the mechanical properties and flame retardant properties are further reduced. In Comparative Example 4, maleic anhydride grafted polyethylene is used as a compatibilizer, and no clay mineral filler is added, so the mechanical properties and flame retardant properties are both the worst.

[0095] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A composite PE plastic, characterized in that: The following raw materials are included by weight: 95-100 parts of high-density polyethylene, 5-10 parts of functional compatibilizer, 2-5.5 parts of modified clay mineral filler, 1-3 parts of lubricant, 0.5-1 parts of antioxidant, and 10-20 parts of pigment and filler; The functional compatibilizer is a low-density polyethylene containing silicon-phosphorus synergistic flame retardant elements and epoxy groups in its structure; The preparation method of the functional compatibilizer comprises the following steps: Step A: low-density polyethylene, (4-vinylphenyl) dimethylsilane, glycidyl methacrylate and benzoyl peroxide are stirred and mixed uniformly, and then added into a torque rheometer, melt-grafted at a temperature of 180-190° C. for 5-10 minutes, and then cooled and discharged to obtain a low-density polyethylene intermediate material; Step B: Add low-density polyethylene intermediate material to xylene, turn on heating until the temperature reaches 80-90°C, stir until completely dissolved, add 2,6,7-trioxa-1-phosphabicyclo (2.2.2) octane-4-methanol-1-oxide and catalyst, after the addition, introduce nitrogen, continue stirring for 4-8 hours, cool and discharge, and obtain a functional compatibilizer; The modified clay mineral filler is illite with branched polyethyleneimine grafted on the surface.

2. A composite PE plastic according to claim 1, characterized in that: The lubricant is any one of paraffin, polyethylene wax, calcium stearate, zinc stearate or stearic acid; the antioxidant is any one of antioxidant 1010, antioxidant 1098 or antioxidant DLTP; the color filler is any one of carbon black or titanium dioxide.

3. A composite PE plastic according to claim 1, characterized in that: In step A, the mass ratio of the low-density polyethylene, (4-vinylphenyl) dimethylsilane, glycidyl methacrylate and benzoyl peroxide is 10:1-2:1.2-2.5:0.05-0.

1.

4. A composite PE plastic according to claim 1, characterized in that: In step A, the catalyst is trifluoroacetic acid.

5. A composite PE plastic according to claim 1, characterized in that: The preparation method of the modified clay mineral filler comprises the following steps: Step A1: After the acidified illite is mixed with toluene to form a uniform dispersion, chlorine-substituted isocyanate and dibutyltin dilaurate are added to the dispersion. After the addition, stirring and heating are started until the system temperature reaches 70-80° C., and after keeping the temperature for 6-12 hours, the solid material is separated to obtain halogenated illite; Step A2: Mix the halogenated illite and 1,4-dioxane, disperse them uniformly by ultrasonication, add branched polyethyleneimine and triethylamine and stir evenly, raise the temperature to 50-60°C, stir at a constant temperature for 4-6 hours, centrifuge the solid product, wash and vacuum dry it, and obtain a modified clay mineral filler.

6. A composite PE plastic according to claim 5, characterized in that: In step A1, the acidification process of the illite is specifically as follows: the illite powder is put into a hydrochloric acid solution with a mass fraction of 1-5%, stirred and mixed, heated to 60-65°C, stirred at a constant temperature for 1-3h, the solid material is separated, washed with deionized water until neutral, and vacuum dried.

7. A composite PE plastic according to claim 5, characterized in that: In step A1, the chlorine-substituted isocyanate is any one of chloroethyl isocyanate or 3-chloropropyl isocyanate.

8. A composite PE plastic according to claim 5, characterized in that: In step A2, the average molecular weight of the branched polyethyleneimine is 10,000.

9. A process for preparing a composite PE plastic according to claim 1, characterized in that: The following steps are involved: Step 1: Weigh each raw material by weight and set aside; Step 2: Pour high-density polyethylene, functional compatibilizer, modified clay mineral filler, lubricant, antioxidant, and pigment filler into a mixer, control the temperature in the mixer to 90-100° C., and stir and mix at a stirring speed of 300-500 r / min for 20-40 minutes to form a premix; Step 3: Place the premix in the extruder, set the temperature of each zone of the extruder as follows: Zone 1 170±5℃, Zone 2 175±5℃, Zone 3 185±5℃, Zone 4 195±5℃, Zone 5 200±5℃, Zone 6 205±5℃, Zone 7 200±5℃, Zone 8 180±5℃, Zone 9 170±5℃, and the die temperature is 165±5℃. After the melt extrusion granulation process, the composite PE plastic can be obtained.

Citation Information

Patent Citations

  • High-performance flame-retardant polyethylene sheath material and preparation method thereof

    CN115678150A

  • Preparation method of phosphorus-nitrogen highly-loaded hydrotalcite flame retardant

    CN109384959A