A photocatalyst for separating technetium or rhenium and its preparation method and application
By simulating sunlight in a polycrystalline titanium dioxide heterophase junction material in a strong acid solution, the problem of low separation efficiency of existing photocatalysts in a strong acid aqueous solution is solved, and high efficiency, stability and environmental protection are achieved separation effect.
Patent Information
- Application Number
- CN202410052716.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-01-12
AI Technical Summary
It is difficult to efficiently separate rhenium or technetium in strongly acidic aqueous solutions, especially when competitive ions are present, the separation efficiency is low, limiting its application in industrial production.
Using polycrystalline titanium dioxide heterophase junction material as photocatalyst, by simulating sunlight to irradiate in a strong acidic solution with pH=1, the built-in electric field and high specific surface area are used to achieve efficient separation of rhenium or technetium. The preparation method includes high pressure Hydrothermal reaction and drying were carried out in the reaction kettle.
In a strong acidic solution with pH=1, the separation efficiency of rhenium is achieved in 6 hours and the material has excellent chemical stability and environmental friendliness, making it suitable for industrial applications.
Smart Images

Figure CN117839666B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of photocatalysis and nuclide separation, and in particular to a photocatalyst for separating technetium or rhenium, and a preparation method and application thereof. Background Art
[0002] Technetium-99 is mainly produced from the thermal neutron-induced fission reaction of uranium-235 and the 238 U spontaneous fission reaction, and the half-life is relatively long (2.13×10 5 Year). 99 Tc also comes from medical isotopes 99m The half-life of Tc decay is only 6.0h. 99 TcO4 - )yes 99 Tc is the most common form in aqueous solution. Because it carries a negative charge, it is difficult to be adsorbed by minerals and sediments in the environment and is easy to migrate, posing a potential threat to the ecological environment. - When it is reduced to low-soluble TcO2·nH2O, it can be separated by filtration, so reduction separation may become a treatment method for Tc in wastewater. Common reducing agents are SO3 2- ,Sn 2+ , Fe 2+ First, when Fe(0) / Fe(II) is used as a reducing agent, it is based on the adsorption-reduction process to fix the 99 Tc / Re. The electrochemical method involves more toxic chemicals, and the presence of SO4 in the aqueous solution 2- It will inhibit the reduction of Re(VII). Although the gamma radiation induced reaction can effectively reduce / separate Re(VII) through hydrated electrons, its experimental conditions are difficult to apply in practice. The removal rate of Re(VII) by photochemical induced reduction (using ultraviolet light or laser irradiation for more than 6 hours) can reach 94.7%, but the high molar absorption rate of Re(VII) limits its treatment concentration level.
[0003] Semiconductor-based heterogeneous photocatalytic reactions and their application in the reduction and removal of heavy metal ions have been reported one after another, such as Cu 2+ , Hg 2+ 、Ag +, U(VI) and Cr(VI). Most photocatalytic materials are considered to be environmentally friendly materials due to their chemical inertness and biocompatibility. Among them, titanium dioxide (TiO2) has the advantages of light corrosion resistance, non-toxicity, low environmental pollution, strong regeneration ability, low cost, and wide sources, and has shown important research value in the field of photocatalytic reduction / removal of metal ions. Compared with traditional chemical reduction methods, photocatalytic reduction itself has the advantages of being clean, efficient, reusable, and easy to recycle. In addition, most photocatalytic materials are a friendly environmental governance strategy due to their chemical inertness and biocompatibility.
[0004] In the research reported so far, it can be used to reduce and separate TcO4 - / ReO4 - The photocatalytic materials are generally poorly active in radioactive highly acidic aqueous solutions, especially in the presence of a large number of competitive ions, and cannot achieve the desired photocatalytic activity on TcO4. - / ReO4 - Therefore, the efficient and selective separation of photocatalysts is limited in industrial production.
[0005] Therefore, it is very necessary to design a photocatalytic material with high photocatalytic efficiency, excellent chemical stability, environmental friendliness and low cost, and its preparation method. Summary of the invention
[0006] The purpose of the present invention is to solve the technical problem that existing photocatalysts (such as P25) cannot efficiently separate rhenium or technetium in strongly acidic aqueous solutions, and to provide a photocatalyst for separating technetium or rhenium and its preparation method and application. The photocatalyst can utilize simulated sunlight to achieve a separation efficiency of more than 80% for rhenium within 6 hours in a strongly acidic solution with a pH of 1.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: a photocatalyst for separating technetium or rhenium, wherein the photocatalyst is a polycrystalline titanium dioxide heterogeneous junction material; the photocatalyst is in powder form, with an average particle size of about 300 to 500 nanometers and a specific surface area of 130 to 240 m 2 ·g -1 .
[0008] The present invention also provides a method for preparing the above-mentioned photocatalyst, comprising the following steps:
[0009] S1, respectively measure ethanol, water and concentrated ammonia water in a volume ratio of 1000:3:6, mix and stir for 5 minutes;
[0010] S2. In the mixed solution of S1, add butyl titanate in an amount of 1 / 50 to 1 / 5 of the volume of ethanol dropwise under vigorous stirring, and then continue stirring for 6-8 hours; then let the precipitate obtained in the solution stand, wash it with ethanol and water alternately for 2-3 times, and filter it;
[0011] S3. Add 60 ml of water to the filtered product, transfer it to a high-pressure reactor lined with polytetrafluoroethylene, and perform hydrothermal reaction at a temperature of 100-200°C for 20 hours. After the reaction is completed, filter it and dry it at 60°C for 24 hours to obtain a polycrystalline titanium dioxide heterogeneous phase material.
[0012] Preferably, the concentration of the concentrated ammonia water in S1 is 28%.
[0013] The present invention also provides the use of the above-mentioned photocatalyst in photocatalytic separation of rhenium or technetium. The photocatalyst is placed in an acidic solution containing rhenium or technetium and irradiated with simulated sunlight for 2 to 6 hours to achieve separation of rhenium or technetium in the solution.
[0014] The beneficial effects of the present invention are as follows: the present invention prepares a photocatalyst of a polycrystalline titanium dioxide heterogeneous junction material, the heterogeneous junction interface of the photocatalyst can form a built-in electric field, drive the migration of photogenerated carriers, reduce the carrier recombination rate, and has a large specific surface area and many reaction sites, thereby effectively improving its photocatalytic separation performance of rhenium or technetium; therefore, the photocatalyst can utilize simulated sunlight to achieve efficient separation of rhenium or technetium in a solution in a strongly acidic solution of pH=1. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the SEM image of the photocatalytic material prepared in Example 1.
[0016] Figure 2 These are the XRD patterns of the photocatalytic materials prepared in Examples 1 and 2.
[0017] Figure 3 This is the TEM image of the photocatalytic material prepared in Example 1.
[0018] Figure 4 This is a nitrogen adsorption and desorption diagram of the photocatalytic material prepared in Example 1.
[0019] Figure 5 The performance of the product of the present invention in removing heavy metal ion rhenium (VII) under simulated sunlight.
[0020] Figure 6 The performance of the product of the present invention in removing heavy metal ions rhenium and technetium under simulated sunlight. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0022] Example 1
[0023] (1) 50 ml of ethanol, 0.15 ml of water, and 0.30 ml of concentrated aqueous ammonia (28%) were measured in a volume ratio of 1000:3:6, mixed, and stirred for 5 minutes;
[0024] (2) Add 5 ml of butyl titanate dropwise to the above solution under vigorous stirring, and then continue stirring for 6 hours;
[0025] (3) The precipitate obtained from the above solution was allowed to stand, washed alternately with ethanol and water for three times, and filtered.
[0026] (4) Add 60 ml of water to the filtered product, transfer it to a high-pressure reactor lined with polytetrafluoroethylene, and perform hydrothermal reaction at 160°C for 20 hours. After the reaction, filter it and dry it at 60°C for 24 hours to obtain a polycrystalline titanium dioxide heterogeneous junction photocatalytic material. The SEM image of the polycrystalline titanium dioxide heterogeneous junction photocatalytic material prepared in this example is shown in the attached figure. Figure 1 As shown, the morphological characteristics of the material can be determined; the XRD diagram is shown in the attached Figure 2 As shown, the existence of heterogeneous phases and the ratio of phases can be determined; TEM images are shown in the attached Figure 3 As shown, it shows a clear heterogeneous existence form; nitrogen adsorption and desorption is shown in the attached figure Figure 4 As shown, the specific surface area is as high as 140.4m 2 / g.
[0027] (5) Photocatalytic experiment: The experimental conditions were to use H2SO4 to make the solution pH = 1 and irradiate with simulated sunlight for 6 hours. The residual amount of rhenium A was detected by inductively coupled plasma emission spectroscopy, A = C t / C0×100%, where C t and C0 represent the concentration of rhenium at a certain moment and the initial moment respectively. The results are as follows Figure 5 shown.
[0028] Example 2
[0029] (1) 50 ml of ethanol, 0.15 ml of water, and 0.30 ml of concentrated aqueous ammonia (28%) were measured in a volume ratio of 1000:3:6, mixed, and stirred for 5 minutes;
[0030] (2) Add 5 ml of butyl titanate dropwise to the above solution under vigorous stirring, and then continue stirring for 6 hours;
[0031] (3) The precipitate obtained from the above solution was allowed to stand, washed twice with ethanol and water alternately, and filtered.
[0032] (4) Add 60 ml of water to the filtered product, transfer it to a high-pressure reactor lined with polytetrafluoroethylene, and perform hydrothermal reaction at 180°C for 20 hours. After the reaction, filter it and dry it at 60°C for 24 hours to obtain a polycrystalline titanium dioxide heterogeneous junction photocatalytic material. The XRD pattern of the polycrystalline titanium dioxide heterogeneous junction photocatalytic material prepared in this embodiment is shown in the attached figure. Figure 2 shown.
[0033] (5) Photocatalytic experiment: The experimental conditions were to use H2SO4 to make the solution pH = 1 and irradiate with simulated sunlight for 6 hours. The residual amount of rhenium A was detected by inductively coupled plasma emission spectroscopy, A = C t / C0×100%, where C t and C0 represent the concentration of rhenium at a certain moment and the initial moment respectively. The results are as follows Figure 5 shown.
[0034] Example 3 Catalyst Competitive Anion Test
[0035] The polycrystalline titanium dioxide heterogeneous junction photocatalytic material prepared in Example 1 was subjected to the following photocatalytic experiment.
[0036] Catalyst competitive anion test: The experimental conditions are to use HClO4 to make the solution pH = 1, add NO 3- , Cl - 、SO4 2- ions and make the concentration 5mmol / L, and then irradiate with simulated sunlight for 6h. The remaining amount of rhenium A was detected by inductively coupled plasma emission spectroscopy, A=C t / C0×100%, where C t and C0 represent the concentration of rhenium at a certain moment and the initial moment respectively. The results are as follows Figure 5 shown.
[0037] Example 4 Catalyst Competitive Cation Test
[0038] The polycrystalline titanium dioxide heterogeneous junction photocatalytic material prepared in Example 1 was subjected to the following photocatalytic experiment.
[0039] Catalyst competitive cation test: The experimental conditions are to use H2SO4 to make the solution pH = 1, add Al 3+ , Cs + , Sr 2+ 、Eu 2+ 、UO2 2+ ions and make the concentration 5mmol / L, and then irradiate with simulated sunlight for 6h. The remaining amount of rhenium A was detected by inductively coupled plasma emission spectroscopy, A=C t / C0×100%, where C tand C0 represent the concentration of rhenium at a certain moment and the initial moment respectively. The results are as follows Figure 5 shown.
[0040] Example 5 Catalyst Separation Test for Rhenium and Technetium
[0041] The polycrystalline titanium dioxide heterogeneous junction photocatalytic material prepared in Example 1 was subjected to the following photocatalytic test: the experimental conditions were to use H2SO4 to make the solution pH = 1, and simulate sunlight irradiation for 2 hours (due to the requirements of radioactivity experiments, only 2 hours were performed, and only 2 hours of data were available). The residual amount of technetium / rhenium A, A = C was detected by liquid scintillation counter and inductively coupled plasma emission spectrometry respectively. t / C0×100%, where C t and C0 represent the concentration of rhenium / technetium at a certain moment and the initial moment respectively. Figure 6 shown.
[0042] In summary, the polycrystalline titanium dioxide heterogeneous junction photocatalytic material prepared by the present invention has excellent photocatalytic performance and can effectively remove the heavy metal ion rhenium (VII).
[0043] The specification and drawings of the present invention are considered to be illustrative rather than restrictive. On the basis of the present invention, those skilled in the art can make some substitutions and modifications to some of the technical features according to the disclosed technical content without creative labor, all of which are within the protection scope of the present invention.
Claims
1. The use of a photocatalyst for separating rhenium or technetium in a strongly acidic solution, characterized in that: The strongly acidic solution is a strongly acidic aqueous solution with a pH of 1; the photocatalyst is placed in a strongly acidic solution containing rhenium or technetium, and irradiated with simulated sunlight for 2 to 6 hours to separate the rhenium or technetium in the solution; The photocatalyst is a polycrystalline titanium dioxide heterogeneous material; the photocatalyst is in powder form, with an average particle size of 300 to 500 nanometers and a specific surface area of 130 to 240 m 2 ·g -1 ; The method for preparing the photocatalyst comprises the following steps: S1, respectively measure ethanol, water and concentrated ammonia water in a volume ratio of 1000:3:6, mix and stir for 5 minutes; S2. In the mixed solution of S1, add butyl titanate in an amount of 1 / 50 to 1 / 5 of the volume of ethanol dropwise under vigorous stirring, and then continue stirring for 6-8 hours; then let the precipitate obtained in the solution stand, wash it with ethanol and water alternately for 2-3 times, and filter it; S3. Add 60 ml of water to the filtered product, transfer it to a high-pressure reactor lined with polytetrafluoroethylene, and perform hydrothermal reaction at a temperature of 100-200°C for 20 hours. After the reaction is completed, filter it and dry it at 60°C for 24 hours to obtain a polycrystalline titanium dioxide heterogeneous phase material.
2. The use according to claim 1, characterized in that: The concentration of the concentrated ammonia water in S1 is 28%.
Citation Information
Cited By
Preparation and application method of photocatalytic material for selective rhenium separation
CN120346802A