Method for preparing high-performance photosensitive solder resist ink based on diamine chain extension modified bisphenol epoxy resin

By using small molecule bisphenol epoxy compounds and diamine chain extension modifiers in photosensitive epoxy resins, combined with acrylic modifiers and acid anhydrides, the resin structure is optimized and the problem of traditional resins being difficult to balance flexibility and media is solved. Solving the problem of electrical properties, the preparation of high-performance photosensitive solder resist ink was achieved.

CN117843921BActive Publication Date: 2024-10-22GUANGDONG YANMO SOLUTION TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311650398.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2024-10-22
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

Traditional printed circuit board (PCB) packaging solder mask UV-modified cured resins are difficult to meet the needs of highly flexible, multi-functional packaging resins, and when pursuing low dielectric constant and other advanced functions, high heat resistance and toughness are often It has been ignored, resulting in brittleness and poor practicality, and it is difficult to balance alkali elution capabilities with mechanical properties.

Method used

A high-performance photosensitive epoxy resin based on chain extension modification of small-molecule bisphenol epoxy compounds is used. Through the combination of diamine chain extension modifier and acrylic modifier, the molar ratio and reaction sequence are optimized to improve the resin quality. The tensile strength, breaking strain, voltage breakdown strength and low dielectric constant, combined with the esterification reaction of acid anhydride, improve the glass transition temperature and alkali development performance.

Benefits of technology

It achieves the improvement of high tensile strength, breaking strain, low dielectric constant and voltage breakdown resistance, ensures the mechanical properties and alkali development performance of the resin, and is suitable for the preparation of high-performance photosensitive solder resist ink.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004587161140000021
    Figure BDA0004587161140000021
  • Figure BDA0004587161140000081
    Figure BDA0004587161140000081
  • Figure BDA0004587161140000101
    Figure BDA0004587161140000101
Patent Text Reader

Abstract

The present invention discloses a method for preparing a high-performance photosensitive solder resist ink based on a diamine chain-extending modified bisphenol epoxy resin, wherein firstly, a high-performance photosensitive epoxy resin based on a small molecule bisphenol epoxy compound chain-extending modified is provided, wherein the high-performance photosensitive epoxy resin is obtained by firstly carrying out a chain-extending reaction between a small molecule bisphenol epoxy compound and a diamine chain-extending modifier, then carrying out a ring-opening reaction with an acrylic modifier, and finally carrying out an esterification reaction with an acid anhydride; secondly, a high-performance photosensitive solder resist ink using the high-performance photosensitive epoxy resin as a main component is provided. In the present invention, by exploring and optimizing the molar ratio of the diamine chain-extending modifier to the small molecule bisphenol epoxy compound, the diamine chain-extending extension unit spatially endows a highly cross-linked conjugated system with an excellent anti-mechanical damping structure, thereby achieving high tensile strength and tensile strain.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photocurable solder resist inks, and relates to a method for preparing a high-performance photosensitive solder resist ink based on a diamine chain-extended modified bisphenol epoxy resin, and specifically relates to a method for preparing a high-performance photosensitive epoxy resin based on a diamine chain-extended modified small molecule bisphenol epoxy compound, and a method for preparing a high-performance photosensitive solder resist ink using the high-performance photosensitive epoxy resin. Background Art

[0002] Customized multifunctional resins with excellent flexibility and high heat resistance have broad prospects in the future advanced semiconductor industry, especially in electronic packaging, 5G communication engineering and the Internet of Things. They are characterized by low cost but provide products that meet specific functional requirements in a precise manner. For example, due to the diversification of application scenarios of 5G wireless communication substrates, higher requirements are put forward in terms of specific customized structures and functions, including low dielectric constants, excellent flexibility and high heat resistance of encapsulation resins / coatings, so as to meet the application in various use environments. However, traditional UV-modified curing resins for printed circuit board (PCB) encapsulation solder mask, such as naphthalene-type, biphenylphenol-type and o-cresol epoxy main chain resins, are difficult to meet the use requirements of preparing highly flexible and multifunctional encapsulation resins / coatings due to their own structural limitations. Therefore, there is an urgent need for a breakthrough in the development of higher-performance photocurable resins that can effectively prepare encapsulation resin products with controllable structures and multifunctionality and meet certain economic practicality. In addition, in order to match the high energy density of integrated circuits and high-speed transmission of electrical signals, it is necessary to ensure that the electronic packaging / coating UV resin must have excellent comprehensive properties, such as excellent tensile strength and toughness, excellent voltage breakdown resistance, weather resistance, and low dielectric properties. In response to these challenges, researchers have made a lot of efforts, such as introducing fluorine atoms with low dielectric properties, doping functionalized modified inorganic nanofillers, and designing three-dimensional void frameworks.

[0003] High glass transition temperature (Tg) and excellent mechanical properties are one of the most competitive properties of photocurable resins, but in the pursuit of low dielectric constants and other advanced functions, high heat resistance and toughness are often overlooked, so they show brittleness, easy to crack due to heat, poor practicality and weather resistance, and their practical applications are greatly limited. At the same time, the alkali elution ability of photocurable resins in packaging applications is crucial for the design of patterned circuits. However, from the perspective of molecular structure design, giving functional resins alkali elution ability will inevitably have a negative impact on the mechanical properties of photocurable resins. Therefore, it is still challenging to balance its microscopic molecular structure and macroscopic properties and develop high-performance photocurable resins with alkali development function.

[0004] Bisphenol A epoxy resin is one of the existing candidates for preparing photosensitive epoxy resins. For example, in the Chinese invention patent "A photosensitive epoxy acrylic resin composition with high toughness and weak alkaline water developability and its preparation method" (CN 107450269 B) of Zhejiang Foster New Materials Research Institute Co., Ltd., the photosensitive resin composition provided has good soldering heat resistance, acid and alkali resistance, solvent resistance, strong adhesion and high bending resistance. The photosensitive resin composition mainly contains: (A) epoxy acrylic resin, (B) tetrahydrophthalic anhydride, tetrahydrofuran acrylate, multifunctional acrylate monomers and nano core-shell rubber toughening resin. Among them, (A) epoxy resin is bisphenol A epoxy resin. However, in the above patents and prior art, macromolecular bisphenol A epoxy resins (mainly oligomers) are basically selected. Therefore, it is very important to provide a method for preparing high-performance photosensitive epoxy resins from a new perspective, and to provide a new type of photocurable solder mask ink with high glass transition temperature, strong toughness, low dielectric constant, and resistance to DC voltage breakdown. Summary of the invention

[0005] In order to solve the problems in the above-mentioned prior art, the present invention provides a method for preparing a high-performance photosensitive solder resist ink based on a diamine chain-extended modified bisphenol epoxy resin. The first invention purpose is to provide a high-performance photosensitive epoxy resin based on a small molecule bisphenol epoxy compound chain-extended modified. The second invention purpose is to provide a method for preparing a high-performance photosensitive solder resist ink using the above-mentioned high-performance photosensitive epoxy resin as a main component.

[0006] To achieve the above objectives, the present invention is implemented by adopting a technical solution consisting of the following technical measures.

[0007] On the one hand, the present invention provides a high-performance photosensitive epoxy resin based on chain extension modification of a small molecule bisphenol epoxy compound, wherein the raw materials thereof mainly include, by molar parts:

[0008]

[0009] Among them, 2 times the molar fraction of the diamine chain extender modifier plus the molar fraction of the acrylic modifier totals 120 parts;

[0010] The small molecule bisphenol epoxy compound is bisphenol A diglycidyl ether or bisphenol F diglycidyl ether.

[0011] Herein, the diamine chain extender modifier is a conventional chain extender having two amino groups, for example, selected from any one of p-phenylenediamine, 4,4'-diaminobiphenyl, 2,2'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4"-diaminoterphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,3-propylenediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,4-butanediol bis(3-aminopropyl) ether, ethylene glycol bis(3-aminopropyl) ether, and bis(3-aminopropyl) ether.

[0012] Furthermore, through comparative experiments, it was found that in the selection of the above-mentioned conventional chain extenders, their chemical structural formulas would significantly affect the performance of the prepared modified epoxy resin. Through the analysis of the experimental results, chain extenders with phenyl, phenoxy, ether, and aromatic ether groups in the chemical structure are preferred, that is, in one of the technical schemes, the diamine chain extender modifier is selected to include any one of p-phenylenediamine, 4,4'-diaminobiphenyl, 2,2'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4"-diamino-p-terphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,4-butanediol bis(3-aminopropyl) ether, ethylene glycol bis(3-aminopropyl) ether, and bis(3-aminopropyl) ether.

[0013] By conducting a horizontal comparison experiment on the above-mentioned preferred diamine chain extender modifiers, it is further preferred that when the diamine chain extender modifier is selected as any one of 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 1,3-bis(4'-aminophenoxy)benzene, and 1,4-butanediol bis(3-aminopropyl) ether, it has significantly better comprehensive properties of the modified epoxy resin (such as high tensile strength, fracture strain, high voltage breakdown strength, and low dielectric constant, etc.); when the diamine chain extender modifier is selected as 1,3-bis(4'-aminophenoxy)benzene, the dynamic thermomechanical properties of the prepared high-performance photosensitive epoxy resin reach the optimal effect, and surprisingly found that its stress-strain performance is significantly better than that of other diamine chain extender modifiers, and is significantly better than 4,4'-diaminodiphenyl ether which also contains phenoxy in its chemical structure, which is beyond the expectations of those skilled in the art.

[0014] In this article, the acrylic modifier is a modifier conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select a suitable acrylic modifier based on the current process conditions or the prior art literature in the art, for example, at least one selected from acrylic acid, 2-furan acrylic acid, 2-thiophene acrylic acid, 3-(3-pyridyl) acrylic acid, 2-acetamido acrylic acid, 4-imidazole acrylic acid, terephthalic acid, trans-3-indole acrylic acid, 2-fluoroacrylic acid, 2-benzyl acrylic acid, hydroxyethyl methacrylate, glycidyl methacrylate, acrylonitrile, and methacrylonitrile.

[0015] In this article, the acid anhydride is a saturated acid anhydride or unsaturated acid anhydride conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select suitable acid anhydrides based on current process conditions or existing technical literature in the art, including monobasic saturated / unsaturated acid anhydrides and polybasic saturated / unsaturated acid anhydrides, and can be selected according to actual process requirements or functional requirements.

[0016] In one of the technical solutions, in order to further improve the cross-linking density of the product, the acid anhydride is preferably a monobasic unsaturated acid anhydride. In the present invention, the monobasic unsaturated acid anhydride is defined as an unsaturated compound having one anhydride group (including a cyclic anhydride formed by dehydration of two carboxyl groups) in its chemical structure, for example, at least one selected from tetrahydrophthalic anhydride, itaconic anhydride, maleic anhydride, methyltetrahydrophthalic anhydride, etc.

[0017] In one technical solution, the acid anhydride is a saturated acid anhydride, selected from at least one of succinic anhydride, phthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

[0018] In one of the technical solutions, in order to make the reaction ratio more balanced, the molar fraction of the acid anhydride is 1 / 2 of the molar fraction of the acrylic modifier.

[0019] It should be noted that the high-performance photosensitive epoxy resin based on the chain extension modification of small molecule bisphenol epoxy compounds mainly includes small molecule bisphenol epoxy compounds, diamine chain extension modifiers, acrylic modifiers, and acid anhydrides. Based on the common knowledge of preparing photosensitive epoxy resins in the art, solvents, catalysts for ring-opening reactions, and inhibitors need to be added during the preparation process. Among them, the catalysts, solvents, and inhibitors for ring-opening reactions are the catalysts, solvents, and inhibitors conventionally selected for preparing photosensitive epoxy resins in the art. Those skilled in the art can select suitable catalysts, solvents, and inhibitors based on the current process conditions or the existing technical literature in the art, or refer to the selection in the following technical scheme.

[0020] In one of the technical solutions, the raw materials may also include fillers and / or additives conventionally used in epoxy resins to achieve further functional expansion / process assistance / enhancement of the product. The specific fillers and / or additives can be selected by those skilled in the art based on the existing technology or existing literature, such as antioxidants, lubricants, carbon-based fillers, coatings, flame retardants, antioxidants, heat stabilizers, coupling agents, plasticizers, compatibilizers, processing aids, etc. It should be noted that the raw materials may include fillers and / or additives conventionally used in epoxy resins, or may not include them.

[0021] One of the inventive points of the present invention is that when a diamine chain extender modifier is used to carry out a chain extension reaction on a small molecule bisphenol epoxy compound, the molar ratio of the two will greatly affect the comprehensive performance of the high-performance photosensitive epoxy resin prepared. This is mainly because the small molecule bisphenol epoxy compound has two epoxy groups in each molecule. After the epoxy group participates in the chain extension reaction, the epoxy group cannot undergo a subsequent ring-opening reaction with the acrylic modifier due to the reduction in the number of epoxy groups. Experiments have found that if the proportion of epoxy groups in the small molecule bisphenol epoxy compound participating in the chain extension reaction is larger, it is easier to affect the viscosity of the intermediate product after chain extension and improve the flexibility of the cured system. However, the epoxy groups that undergo a subsequent ring-opening reaction with the acrylic modifier are reduced, which has a negative impact on the photocuring efficiency, the curing crosslinking density and the glass transition temperature of the resin. The formula ratio provided in the technical solution of the present invention greatly balances the contradiction between the two, thereby having a high-performance technical effect, and providing a foundation for the subsequent preparation of photosensitive epoxy resins using small molecule epoxy compounds for chain extension.

[0022] The above technical scheme provides a high-performance photosensitive epoxy resin based on chain extension modification of small molecule bisphenol epoxy compounds, and gives its main raw material composition. Based on the common knowledge in the field, those skilled in the art can know the conventional process of chain extension reaction and the conventional modification preparation method of photosensitive epoxy resin.

[0023] However, it should be noted that the experiment found that the addition method and reaction order of the diamine chain extender and acrylic modifier will have a certain degree of impact on the industrial preparation yield of the final product. First, although the epoxy group can undergo chain extension and ring opening reactions at the same time, if the diamine chain extender and acrylic modifier are added to participate in the reaction at the same time, there is a competitive reaction between the two and the epoxy group, resulting in a decrease in the yield of the desired product and the generation of side reaction products. Secondly, the question of whether to choose a diamine chain extender or an acrylic modifier in the first step of the reaction. From the perspective of industrial production, the selection of a diamine chain extender in the first step of the reaction can confirm the specific structure after chain extension through detection methods such as nuclear magnetic resonance, which is conducive to standardizing the required modified epoxy resin and exploring more suitable process conditions through sample production and actual production processes.

[0024] Based on the above description, in one of the technical solutions, the high-performance photosensitive epoxy resin is first obtained by a chain extension reaction between a small molecule bisphenol epoxy compound and a diamine chain extender modifier, then a ring-opening reaction with an acrylic modifier, and finally an esterification reaction with an acid anhydride.

[0025] In order to better illustrate the present invention and provide a preferred technical solution, the above-mentioned method for preparing a high-performance photosensitive epoxy resin based on chain extension modification of a small molecule bisphenol epoxy compound mainly comprises the following steps:

[0026] (1) In an air atmosphere, preheat the solvent to 75-95° C., add a small molecular bisphenol epoxy compound and dissolve it, cool it to 55-65° C., add a diamine chain extender modifier, then heat it to 75-95° C., add a catalyst for a ring-opening reaction, and then adjust the temperature to 85-95° C., stir and react for 4-6 hours until the acid value of the reaction solution is less than 3 mgKOH / g, thereby obtaining a chain-extended modified epoxy resin solution;

[0027] (2) cooling the chain-extended epoxy resin solution obtained in step (1) to 55-65° C., then adding an acrylic modifier, a catalyst for a ring-opening reaction and a polymerization inhibitor, and stirring the mixture at 100-110° C. for 8-12 hours until the acid value of the reaction solution is less than 3 mgKOH / g, adjusting the temperature to 70-90° C., adding a polymerization inhibitor and anhydride, and then adjusting the temperature to 95-105° C. and stirring the mixture for 6-8 hours to prepare a high-performance photosensitive epoxy resin.

[0028] Herein, the solvent described in step (1) is a solvent conventionally selected in the art for preparing photosensitive epoxy resins. A person skilled in the art can select a suitable solvent, such as a conventional organic solvent, based on the current process conditions or prior art literature in the art. The solvent can be selected according to actual process requirements or functional requirements.

[0029] In one of the technical schemes, the solvent in step (1) is preferably at least one of a dibasic acid ester high-boiling point environmentally friendly solvent, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ether, propylene glycol methyl ether, trimethylbenzene and tetramethylbenzene; in step (1), the mass of the solvent: the mass of the small molecule bisphenol epoxy compound = (0.5~1.5): 1.

[0030] In one of the technical solutions, in step (1), in order to improve the reaction efficiency and reduce the loss caused by the reactants sticking to the wall of the reaction container, the diamine chain extender modifier can be first dissolved in an appropriate amount of solvent and then added; the solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0031] In one of the technical solutions, in step (2), in order to improve the reaction efficiency and reduce the loss caused by the reactants sticking to the wall of the reaction container, the acrylic modifier can be dissolved in a suitable amount of solvent before adding it; the solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0032] In one of the technical solutions, in the step (1) and (2), the catalyst for the ring-opening reaction is added. In order to improve the reaction efficiency and reduce the loss caused by the reactants sticking to the wall of the reaction container, the catalyst for the ring-opening reaction can be dissolved in a suitable amount of solvent before adding. The solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0033] In one of the technical solutions, in step (2), in order to improve the reaction efficiency and reduce the loss caused by the solid reactants sticking to the wall of the reaction container, the inhibitor can be dissolved in a suitable amount of solvent before adding it; the solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0034] In one of the technical solutions, in step (2), in order to improve the reaction efficiency and reduce the loss caused by the solid reactants sticking to the wall of the reaction container, the acid anhydride can be dissolved in a suitable amount of solvent before adding it; the solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0035] Herein, the polymerization inhibitor in step (2) is a polymerization inhibitor conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select a suitable polymerization inhibitor based on current process conditions or existing technical literature in the art.

[0036] In one of the technical solutions, the polymerization inhibitor in step (2) is preferably at least one of hydroquinone, o-methyl hydroquinone, p-hydroxyanisole, p-benzoquinone and 2,6-di-tert-butyl-4-methylphenol. Preferably, the polymerization inhibitor added twice is the same polymerization inhibitor, and the amount of the polymerization inhibitor added each time is 0.4 to 1.5 wt% of the small molecular bisphenol epoxy compound in step (1).

[0037] Herein, the catalyst for the ring-opening reaction in step (2) is a catalyst for the ring-opening reaction conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select a suitable catalyst for the ring-opening reaction based on the current process conditions or the prior art literature in the art.

[0038] In one of the technical solutions, the catalyst for the ring-opening reaction in step (2) is selected from any one of triethylamine, triethanolamine, 4-dimethylaminopyridine, tetrabutylammonium bromide, tetramethylammonium chloride, N,N-dimethylbenzylamine and triphenylphosphine; the amount of the catalyst added for the ring-opening reaction is 0.2 to 1 wt% of the small molecule bisphenol epoxy compound in step (1).

[0039] Herein, the stirring reaction in steps (1) and (2) is a stirring reaction conventionally used in the art, including magnetic stirring or mechanical stirring, and those skilled in the art can select a suitable stirring reaction mode according to the production scale or the current process conditions. In order to better illustrate the present invention and provide a process scheme suitable for a laboratory operating environment, the stirring reaction can be carried out at a stirring rate of 100 to 400 rpm.

[0040] On the other hand, the present invention also provides a high-performance photosensitive solder resist ink using the above-mentioned high-performance photosensitive epoxy resin as a main component, and its raw materials mainly include, by weight:

[0041] 100 parts of high performance photosensitive epoxy resin,

[0042] 2 to 5 parts of photoinitiator.

[0043] Herein, the photoinitiator is a photoinitiator conventionally selected for preparing photosensitive solder resist ink in the art, and those skilled in the art can select a suitable photoinitiator based on the current process conditions or existing technical literature in the art.

[0044] In one of the technical solutions, the photoinitiator is preferably at least one of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2-hydroxy-4-(2-hydroxyethoxyphenyl)-2-methylpropiophenone, 2-isopropylthioxanthone (2,4 isomers), 2-hydroxy-2-methyl-1-phenylpropiophenone, 1-hydroxycyclohexylphenylmethanol, benzoin ethyl ether, benzil dimethyl ketal, 1-hydroxyphenylhexylacetophenone, benzophenone / triethanolamine and benzophenone / acrylate active amine.

[0045] In one preferred technical solution, the high-performance photosensitive solder resist ink mainly comprises, by weight:

[0046]

[0047] Among them, in order to improve the physical strength of the coating after the solder resist ink is used, the solder resist ink component includes a filler, and the filler is a well-known inorganic or organic filler, preferably one or more of titanium dioxide, bentonite, barium sulfate, spherical silica, nano calcium carbonate, and talc. Furthermore, it is preferred that well-known metal oxides are used as both fillers and pigments.

[0048] The additive is one or more combinations of pigments, thermal inhibitors, tackifiers, defoamers, leveling agents, coupling agents, antioxidants and rust inhibitors. Generally, the pigments, thermal inhibitors, tackifiers, defoamers, leveling agents, coupling agents, antioxidants and rust inhibitors are well known and commonly used.

[0049] The preparation method of the high-performance photosensitive solder resist ink can be prepared by mixing all components in accordance with the prior art. For example, the components are preliminarily mixed in a blender and then kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0050] When the solder resist ink is used, it is applied to the substrate, dried appropriately (about 60 to 100°C), and then exposed to ultraviolet light for 30 to 120 seconds to obtain a cured coating. Preferably, the photocured coating is further cured by heat treatment at 130 to 180°C for 45 to 75 minutes.

[0051] Generally, the high-performance photosensitive solder resist ink can be directly applied to a substrate in a liquid state or used in a state of a solder resist layer dry film formed by applying and drying on a film such as PET in advance.

[0052] The present invention has the following beneficial effects:

[0053] (1) The present invention provides a high-performance photosensitive epoxy resin based on chain extension modification of a small molecule bisphenol epoxy compound, wherein a small molecule bisphenol epoxy compound is chain extended by a diamine chain extender modifier, and a designed amount of chain extension epoxy units are introduced in the first amino ring-opening reaction, and a functionalized intermediate extension structure is introduced at both ends of the compound by an esterification reaction of a diamine group and epoxy, so that the intermediate product after the chain extension has a higher degree of freedom and has different numbers of rigid benzene ring structures and flexible long carbon chain fatty ether structures connected by ether bonds, which significantly promotes the mechanical properties and other properties of the high-performance photosensitive epoxy resin finally obtained.

[0054] (2) In the present invention, by exploring and optimizing the molar ratio of the diamine chain extender modifier to the small molecule bisphenol epoxy compound, the diamine chain extender extension unit is spatially endowed with an excellent anti-mechanical damping structure of the highly cross-linked conjugated system, thereby achieving high tensile strength and tensile strain.

[0055] (3) In one of the technical solutions, a large number of hydroxyl groups are introduced through the ring-opening reaction, and a higher proportion of unsaturated acid anhydride is also added. A large number of unsaturated double bonds and carboxyl groups are introduced by the esterification reaction of the hydroxyl group and the acid anhydride, thereby ensuring a high double bond density of the obtained high-performance photosensitive epoxy resin. Therefore, the film has a higher glass transition temperature after curing.

[0056] (4) In the present invention, a large number of carboxyl groups are introduced by reacting anhydride with hydroxyl groups, so that the product has good alkali developing performance, and can be quickly and completely detached by directly immersing in concentrated alkali solution without damaging the substrate.

[0057] (5) The high-performance photosensitive solder resist ink prepared by the high-performance photosensitive epoxy resin provided by the present invention has excellent performance in terms of mechanical properties, dielectric properties, voltage breakdown resistance, and electrical insulation properties after testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 The following are hydrogen nuclear magnetic spectra of the products of each step in the preparation process of Synthesis Examples 1 to 4 of the present invention. The products of each step in the preparation process are named X-BA1, X-BA2 and X-BA, respectively, X is the initials of the English abbreviations of different diamine chain extenders, the number 1 refers to the epoxy resin modified by chain extension obtained in step (1), that is, the product extended by the diamine chain extender; the number 2 refers to the product obtained after the reaction with acrylic acid in step (2); the product without a number is the abbreviation of the final product, that is, the product obtained after the reaction with anhydride.

[0059] Figure 2 This is a comparison chart of tan (δ), storage modulus, loss modulus, stress-strain and related toughness curves of the high-performance photosensitive solder resist ink finally prepared in Examples 1 to 4 of the present invention as samples after curing.

[0060] Figure 3 The stress-strain curve comparison diagram of the high-performance photosensitive solder resist ink finally prepared in Examples 3, 5, and 6 of the present invention after curing as a sample. In the figure, P-BA-20% is the sample of Example 6, P-BA-10% is the sample of Example 3, and P-BA-5% is the sample of Example 5.

[0061] Figure 4 The dielectric constant comparison spectra of the high-performance photosensitive solder resist inks finally prepared in Examples 3, 5, and 6 of the present invention after curing are used as samples. In the figure, P-BA-20 is the sample of Example 6, P-BA-10 is the sample of Example 3, and P-BA-5 is the sample of Example 5.

[0062] Figure 5The DC voltage breakdown strength comparison chart of the photosensitive solder resist ink finally prepared in Examples 3, 5, 6 of the present invention and Comparative Example 1 after curing is used as a sample. In the figure, P-BA-20% is the sample of Example 6, P-BA-10% is the sample of Example 3, P-BA-5% is the sample of Example 5, and BA is the sample of Comparative Example 1.

[0063] Figure 6 The following is a comparison chart of the glass transition temperatures of the photosensitive solder resist inks finally prepared in Examples 3, 5, 6 and Comparative Example 1 of the present invention after curing as samples. In the figure, P-BA-20% is the sample of Example 6, P-BA-10% is the sample of Example 3, P-BA-5% is the sample of Example 5, and BA is the sample of Comparative Example 1. DETAILED DESCRIPTION

[0064] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously change or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention. Although it is believed that those of ordinary skill in the art fully understand the following terms, the following definitions are still stated to help illustrate the subject matter disclosed by the present invention.

[0065] On the one hand, the present invention provides a high-performance photosensitive epoxy resin based on chain extension modification of a small molecule bisphenol epoxy compound, wherein the raw materials thereof mainly include, by mole fraction:

[0066]

[0067] Among them, 2 times the molar fraction of the diamine chain extender modifier plus the molar fraction of the acrylic modifier totals 120 parts;

[0068] The small molecule bisphenol epoxy compound is bisphenol A diglycidyl ether or bisphenol F diglycidyl ether.

[0069] Herein, the diamine chain extender modifier is a conventional chain extender having two amino groups, for example, selected from any one of p-phenylenediamine, 4,4'-diaminobiphenyl, 2,2'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4"-diaminoterphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,3-propylenediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,4-butanediol bis(3-aminopropyl) ether, ethylene glycol bis(3-aminopropyl) ether, and bis(3-aminopropyl) ether.

[0070] Furthermore, through comparative experiments, it was found that in the selection of the above-mentioned conventional chain extenders, their chemical structural formulas would significantly affect the properties of the prepared modified epoxy resin. Through the analysis of the experimental results, chain extenders with phenyl, phenoxy, ether, and aromatic ether groups in the chemical structure are preferred, that is, in one embodiment, the diamine chain extender modifier is selected to include any one of p-phenylenediamine, 4,4'-diaminobiphenyl, 2,2'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4"-diaminoterphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,4-butanediol bis(3-aminopropyl) ether, ethylene glycol bis(3-aminopropyl) ether, and bis(3-aminopropyl) ether.

[0071] In one embodiment, by conducting a horizontal comparison experiment on the above-mentioned preferred diamine chain extender modifier, it is further preferred to find that when the diamine chain extender modifier is selected as any one of 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 1,3-bis(4'-aminophenoxy)benzene, and 1,4-butanediol bis(3-aminopropyl) ether, it has significantly better comprehensive properties of the modified epoxy resin (such as high tensile strength, fracture strain, high voltage breakdown strength, and low dielectric constant, etc.); when the diamine chain extender modifier is selected as 1,3-bis(4'-aminophenoxy)benzene, the dynamic thermomechanical properties of the prepared high-performance photosensitive epoxy resin reach the optimal effect, and surprisingly found that its stress-strain performance is significantly better than that of other diamine chain extender modifiers, and is significantly better than 4,4'-diaminodiphenyl ether which also contains phenoxy in its chemical structure, which is beyond the expectations of those skilled in the art.

[0072] In one embodiment, the diamine chain extender modifier is 3 to 22 parts, for example, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts or any range or point value therebetween.

[0073] In this article, the acrylic modifier is a modifier conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select a suitable acrylic modifier based on the current process conditions or the prior art literature in the art. In one embodiment, for example, it is selected from at least one of acrylic acid, 2-furan acrylic acid, 2-thiophene acrylic acid, 3-(3-pyridyl) acrylic acid, 2-acetamido acrylic acid, 4-imidazole acrylic acid, terephthalic acid, trans-3-indole acrylic acid, 2-fluoroacrylic acid, 2-benzyl acrylic acid, hydroxyethyl methacrylate, glycidyl methacrylate, acrylonitrile, and methacrylonitrile.

[0074] In one embodiment, the acrylic modifier is 76 to 114 parts, for example, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114 parts, or any range or point value therebetween.

[0075] In this article, the acid anhydride is a saturated acid anhydride or unsaturated acid anhydride conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select suitable acid anhydrides based on current process conditions or existing technical literature in the art, including monobasic saturated / unsaturated acid anhydrides and polybasic saturated / unsaturated acid anhydrides, and can be selected according to actual process requirements or functional requirements.

[0076] In one embodiment, in order to further improve the cross-linking density of the product, the acid anhydride is preferably a monobasic unsaturated acid anhydride. In the present invention, the monobasic unsaturated acid anhydride is defined as an unsaturated compound having one anhydride group (including a cyclic anhydride formed by dehydration of two carboxyl groups) in its chemical structure, for example, at least one selected from tetrahydrophthalic anhydride, itaconic anhydride, maleic anhydride, methyltetrahydrophthalic anhydride, etc.

[0077] In one embodiment, the acid anhydride is a saturated acid anhydride, selected from at least one of succinic anhydride, phthalic anhydride, hexahydrophthalic anhydride and methylhexahydrophthalic anhydride.

[0078] In one embodiment, in order to make the reaction ratio more balanced, the molar fraction of the acid anhydride is 1 / 2 of the molar fraction of the acrylic modifier.

[0079] In one embodiment, the anhydride is 38 to 57 parts, for example, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57 parts or any range or point value therebetween.

[0080] It should be noted that the high-performance photosensitive epoxy resin based on the chain extension modification of small molecule bisphenol epoxy compounds mainly includes small molecule bisphenol epoxy compounds, diamine chain extension modifiers, acrylic modifiers, and acid anhydrides. Based on the common knowledge of preparing photosensitive epoxy resins in the art, solvents, catalysts for ring-opening reactions, and inhibitors need to be added during the preparation process. Among them, the catalysts, solvents, and inhibitors for ring-opening reactions are the catalysts, solvents, and inhibitors conventionally selected for preparing photosensitive epoxy resins in the art. Those skilled in the art can select suitable catalysts, solvents, and inhibitors based on the current process conditions or the existing technical literature in the art, or refer to the selection in the following technical scheme.

[0081] In one embodiment, the raw material may also include fillers and / or additives conventionally used in epoxy resins to achieve further functional expansion / process assistance / enhancement of the product. The specific fillers and / or additives can be selected by those skilled in the art based on the prior art or existing literature, such as antioxidants, lubricants, carbon-based fillers, coatings, flame retardants, antioxidants, thermal stabilizers, coupling agents, plasticizers, compatibilizers, processing aids, etc. Note that the raw material may include fillers and / or additives conventionally used in epoxy resins, or may not include them.

[0082] One of the inventive points of the present invention is that when a diamine chain extender modifier is used to carry out a chain extension reaction on a small molecule bisphenol epoxy compound, the molar ratio of the two will greatly affect the comprehensive performance of the high-performance photosensitive epoxy resin prepared. This is mainly because the small molecule bisphenol epoxy compound has two epoxy groups in each molecule. After the epoxy group participates in the chain extension reaction, the epoxy group cannot undergo a subsequent ring-opening reaction with the acrylic modifier due to the reduction in the number of epoxy groups. Experiments have found that if the proportion of epoxy groups in the small molecule bisphenol epoxy compound participating in the chain extension reaction is larger, it is easier to affect the viscosity of the intermediate product after chain extension and improve the flexibility of the cured system. However, the epoxy groups that undergo a subsequent ring-opening reaction with the acrylic modifier are reduced, which has a negative impact on the photocuring efficiency, the curing crosslinking density and the glass transition temperature of the resin. The formula ratio provided in the technical solution of the present invention greatly balances the contradiction between the two, thereby having a high-performance technical effect, and providing a foundation for the subsequent preparation of photosensitive epoxy resins using small molecule epoxy compounds for chain extension.

[0083] The above technical scheme provides a high-performance photosensitive epoxy resin based on chain extension modification of small molecule bisphenol epoxy compounds, and gives its main raw material composition. Based on the common knowledge in the field, those skilled in the art can know the conventional process of chain extension reaction and the conventional modification preparation method of photosensitive epoxy resin.

[0084] However, it should be noted that the experiment found that the addition method and reaction order of the diamine chain extender and acrylic modifier will have a certain degree of impact on the industrial preparation yield of the final product. First, although the epoxy group can undergo chain extension and ring opening reactions at the same time, if the diamine chain extender and acrylic modifier are added to participate in the reaction at the same time, there is a competitive reaction between the two and the epoxy group, resulting in a decrease in the yield of the desired product and the generation of side reaction products. Secondly, the question of whether to choose a diamine chain extender or an acrylic modifier in the first step of the reaction. From the perspective of industrial production, the selection of a diamine chain extender in the first step of the reaction can confirm the specific structure after chain extension through detection methods such as nuclear magnetic resonance, which is conducive to standardizing the required modified epoxy resin and exploring more suitable process conditions through sample production and actual production processes.

[0085] Based on the above description, in one embodiment, the high-performance photosensitive epoxy resin is obtained by firstly performing a chain extension reaction between a small molecule bisphenol epoxy compound and a diamine chain extender modifier, then performing a ring-opening reaction with an acrylic modifier, and finally performing an esterification reaction with an acid anhydride.

[0086] In order to better illustrate the present invention and provide a preferred embodiment, the above-mentioned method for preparing a high-performance photosensitive epoxy resin based on chain extension modification of a small molecule bisphenol epoxy compound mainly comprises the following steps:

[0087] (1) In an air atmosphere, preheat the solvent to 75-95° C., add a small molecular bisphenol epoxy compound and dissolve it, cool it to 55-65° C., add a diamine chain extender modifier, then heat it to 75-95° C., add a catalyst for a ring-opening reaction, and then adjust the temperature to 85-95° C., stir and react for 4-6 hours until the acid value of the reaction solution is less than 3 mgKOH / g, thereby obtaining a chain-extended modified epoxy resin solution;

[0088] (2) cooling the chain-extended epoxy resin solution obtained in step (1) to 55-65° C., then adding an acrylic modifier, a catalyst for a ring-opening reaction and a polymerization inhibitor, and stirring the mixture at 100-110° C. for 8-12 hours until the acid value of the reaction solution is less than 3 mgKOH / g, adjusting the temperature to 70-90° C., adding a polymerization inhibitor and anhydride, and then adjusting the temperature to 95-105° C. and stirring the mixture for 6-8 hours to prepare a high-performance photosensitive epoxy resin.

[0089] Herein, the solvent described in step (1) is a solvent conventionally selected in the art for preparing photosensitive epoxy resins. A person skilled in the art can select a suitable solvent, such as a conventional organic solvent, based on the current process conditions or prior art literature in the art. The solvent can be selected according to actual process requirements or functional requirements.

[0090] In one embodiment, the solvent in step (1) is preferably at least one of a dibasic acid ester high boiling point environmentally friendly solvent, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ether, propylene glycol methyl ether, trimethylbenzene and tetramethylbenzene; in step (1), solvent mass: small molecule bisphenol epoxy compound mass = (0.5-1.5): 1, for example 0.5: 1, 0.6: 1, 0.7: 1, 0.8: 1, 0.9: 1, 1: 1, 1.1: 1, 1.2: 1, 1.3: 1, 1.4: 1, 1.5: 1 or any range or point value therebetween.

[0091] In one embodiment, in step (1), in order to improve the reaction efficiency and reduce the loss caused by the reactants sticking to the wall of the reaction container, the diamine chain extender modifier can be first dissolved in a suitable amount of solvent and then added; the solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0092] In one embodiment, in step (2), in order to improve the reaction efficiency and reduce the loss caused by the reactants sticking to the wall of the reaction container, the acrylic modifier can be dissolved in a suitable amount of solvent before adding. The solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0093] In one embodiment, in the step (1) and (2), in order to improve the reaction efficiency and reduce the loss caused by the reactants sticking to the wall of the reaction container, the catalyst for the ring-opening reaction can be dissolved in a suitable amount of solvent before adding. The solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0094] In one embodiment, in step (2), in order to improve the reaction efficiency and reduce the loss caused by the solid reactants sticking to the wall of the reaction container, the inhibitor can be dissolved in a suitable amount of solvent before adding. The solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0095] In one embodiment, in step (2), in order to improve the reaction efficiency and reduce the loss caused by the solid reactants sticking to the wall of the reaction container, the acid anhydride can be first dissolved in a suitable amount of solvent and then added; the solvent can be the same solvent as the above-mentioned small molecule bisphenol epoxy compound.

[0096] Herein, the polymerization inhibitor in step (2) is a polymerization inhibitor conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select a suitable polymerization inhibitor based on current process conditions or existing technical literature in the art.

[0097] In one embodiment, the inhibitor in step (2) is preferably at least one of hydroquinone, o-methyl hydroquinone, p-hydroxyanisole, p-benzoquinone and 2,6-di-tert-butyl-4-methylphenol. Preferably, the inhibitor added twice is the same inhibitor, and the amount of the inhibitor added each time is 0.4-1.5wt% of the small molecule bisphenol epoxy compound in step (1), such as 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt% or any range or point value therebetween.

[0098] Herein, the catalyst for the ring-opening reaction in step (2) is a catalyst for the ring-opening reaction conventionally selected in the art for preparing photosensitive epoxy resins. Those skilled in the art can select a suitable catalyst for the ring-opening reaction based on the current process conditions or the prior art literature in the art.

[0099] In one embodiment, the catalyst for the ring-opening reaction in step (2) is selected from any one of triethylamine, triethanolamine, 4-dimethylaminopyridine, tetrabutylammonium bromide, tetramethylammonium chloride, N,N-dimethylbenzylamine and triphenylphosphine; the amount of the catalyst added in the ring-opening reaction is 0.2-1wt% of the small molecule bisphenol epoxy compound in step (1), for example, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt% or any range or point value therebetween.

[0100] Herein, the stirring reaction in steps (1) and (2) is a stirring reaction conventionally used in the art, including magnetic stirring or mechanical stirring, and those skilled in the art can select a suitable stirring reaction mode according to the production scale or the current process conditions. In order to better illustrate the present invention and provide a process scheme suitable for a laboratory operating environment, the stirring reaction can be carried out at a stirring rate of 100 to 400 rpm.

[0101] On the other hand, the present invention also provides a high-performance photosensitive solder resist ink using the above-mentioned high-performance photosensitive epoxy resin as a main component, and its raw materials mainly include, by weight:

[0102] 100 parts of high performance photosensitive epoxy resin,

[0103] 2 to 5 parts of photoinitiator.

[0104] Herein, the photoinitiator is a photoinitiator conventionally selected for preparing photosensitive solder resist ink in the art, and those skilled in the art can select a suitable photoinitiator based on the current process conditions or existing technical literature in the art.

[0105] In one embodiment, the photoinitiator is preferably at least one of 2,4,6-(trimethylbenzoyl)diphenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2-hydroxy-4-(2-hydroxyethoxyphenyl)-2-methylpropiophenone, 2-isopropylthioxanthone (2,4 isomers), 2-hydroxy-2-methyl-1-phenylpropiophenone, 1-hydroxycyclohexylphenylmethanol, benzoin ethyl ether, benzil dimethyl ketal, 1-hydroxyphenylhexylacetophenone, benzophenone / triethanolamine and benzophenone / acrylate active amine.

[0106] In one preferred embodiment, the high-performance photosensitive solder resist ink mainly comprises, by weight:

[0107]

[0108] Among them, in order to improve the physical strength of the coating after the solder resist ink is used, the solder resist ink component includes a filler, and the filler is a well-known inorganic or organic filler. In one embodiment, one or more of titanium dioxide, bentonite, barium sulfate, spherical silica, nano-calcium carbonate, and talc are preferred. Furthermore, well-known metal oxides are preferably used as both fillers and pigments.

[0109] In one embodiment, the additive is one or more combinations of pigments, thermal inhibitors, tackifiers, defoamers, leveling agents, coupling agents, antioxidants and rust inhibitors. Generally, the above-mentioned pigments, thermal inhibitors, tackifiers, defoamers, leveling agents, coupling agents, antioxidants and rust inhibitors are well-known and commonly used.

[0110] The preparation method of the high-performance photosensitive solder resist ink can be prepared by mixing all components in accordance with the prior art. For example, the components are preliminarily mixed in a blender and then kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0111] When the solder resist ink is used, it is applied to the substrate, dried appropriately (about 60 to 100°C), and then exposed to ultraviolet light for 30 to 120 seconds to obtain a cured coating. Preferably, the photocured coating is further cured by heat treatment at 130 to 180°C for 45 to 75 minutes.

[0112] Generally, the high-performance photosensitive solder resist ink can be directly applied to a substrate in a liquid state or used in a state of a solder resist layer dry film formed by applying and drying on a film such as PET in advance.

[0113] In one embodiment, the filler is 25 to 45 parts, for example, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts or any range or point value therebetween.

[0114] In one embodiment, the additive is 1 to 20 parts, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or any range or point value therebetween.

[0115] The present invention will be further explained in detail with reference to the following examples. However, it should be understood by those skilled in the art that these examples are provided for illustrative purposes only and are not intended to limit the present invention.

[0116] Example

[0117] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. The specific conditions not specified in the examples are carried out according to the conditions recommended by normal conditions or manufacturers. The reagents used or the instruments not specified by the manufacturer are all conventional products that can be obtained commercially. The application should not be construed as being limited to the specific examples described.

[0118] 1. Raw materials

[0119] Bisphenol A diglycidyl ether (DGEBA) (≥85%) was purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0120] p-Phenylenediamine (pP), 4,4′-diaminodiphenylmethane (DDM), and 4,4′-diaminodiphenyl ether (ODA) were provided by Adamas-beta Biotechnology Co., Ltd., 1,4-butanediol bis(3-aminopropyl) ether (BEA) was purchased from Aladdin Reagent (Shanghai) Co., Ltd., China, and 1,3-bis(4′-aminophenoxy)benzene (TPER) was purchased from Shanghai McLean Biochemical Co., Ltd.

[0121] Hydroquinone (HQ), triphenylphosphine (TPP), 4-dimethylaminopyridine (DMAP), and diethylene glycol ethyl ether acetate (DCAC) were from Huaxia Reagent Co., Ltd. (Chengdu, China).

[0122] Acrylic acid (AA), tetrahydrophthalic anhydride (THPA) and photoinitiator 2-isopropylthioxanthone (ITX) were provided by Sinopharm Chemical Reagent Co., Ltd.

[0123] Synthesis example 1

[0124] Synthesis Example 1 is to prepare a high-performance photosensitive epoxy resin based on chain extension modification of a small molecular bisphenol epoxy compound, and its raw materials mainly include, by mole:

[0125]

[0126] The diamine chain extender modifier is 4,4'-diaminodiphenylmethane.

[0127] The preparation method of the high-performance photosensitive epoxy resin comprises the following steps:

[0128] (1) In an air atmosphere, preheat the solvent diethylene glycol ethyl ether acetate to 80° C., add bisphenol A diglycidyl ether and dissolve it, cool it to 60° C., add a diamine chain extender modifier, then heat it to 90° C., add triphenylphosphine as a catalyst for the ring-opening reaction, maintain the temperature at 90° C., and stir the reaction for 6 hours to obtain a chain-extended epoxy resin solution;

[0129] The mass of solvent diethylene glycol ethyl ether acetate: mass of bisphenol A diglycidyl ether = 1:1, and the amount of catalyst triphenylphosphine added for ring-opening reaction is 0.8wt% of the bisphenol A diglycidyl ether;

[0130] (2) cooling the chain-extended epoxy resin solution obtained in step (1) to 60° C., then adding acrylic acid, a ring-opening reaction catalyst triphenylphosphine and a polymerization inhibitor hydroquinone, and mixing, continuing to stir and react at 110° C. for 10 hours until the acid value of the reaction solution is less than 3 mgKOH / g, adjusting the temperature to 80° C., adding a polymerization inhibitor hydroquinone and tetrahydrophthalic anhydride, and mixing, and then adjusting the temperature to 100° C., stirring and reacting for 6 hours to prepare a high-performance photosensitive epoxy resin, denoted as D-BA;

[0131] The amount of triphenylphosphine as a catalyst for the ring-opening reaction is 0.8 wt % of the bisphenol A diglycidyl ether in step (1).

[0132] The amount of the polymerization inhibitor hydroquinone added each time is 0.4 wt % of the small molecular bisphenol epoxy compound in step (1).

[0133] Synthesis example 2

[0134] In Synthesis Example 2, 4,4'-diaminodiphenyl ether is used as a diamine chain extender modifier, and the rest is consistent with the implementation of Synthesis Example 1 to prepare a high-performance photosensitive epoxy resin, which is denoted as O-BA.

[0135] Synthesis example 3

[0136] In Synthesis Example 3, 1,3-bis(4'-aminophenoxy)benzene is used as a diamine chain extender modifier, and the rest is consistent with the implementation of Synthesis Example 1 to prepare a high-performance photosensitive epoxy resin, which is denoted as P-BA.

[0137] Synthesis example 4

[0138] In Synthesis Example 4, 1,4-butanediol bis(3-aminopropyl) ether was used as a diamine chain extender modifier, and the rest was consistent with the implementation of Synthesis Example 1 to prepare a high-performance photosensitive epoxy resin, which was recorded as B-BA.

[0139] Synthesis example 5

[0140] Synthesis Example 5 is to prepare a high-performance photosensitive epoxy resin based on chain extension modification of a small molecular bisphenol epoxy compound, and its raw materials mainly include, by mole:

[0141]

[0142] The diamine chain extender modifier is 1,3-bis(4'-aminophenoxy)benzene.

[0143] The preparation method of the high-performance photosensitive epoxy resin comprises the following steps:

[0144] (1) In an air atmosphere, preheat the solvent diethylene glycol ethyl ether acetate to 80° C., add bisphenol A diglycidyl ether and dissolve it, cool it to 60° C., add a diamine chain extender modifier, then heat it to 90° C., add triphenylphosphine as a catalyst for the ring-opening reaction, maintain the temperature at 90° C., and stir the reaction for 6 hours to obtain a chain-extended epoxy resin solution;

[0145] The mass of solvent diethylene glycol ethyl ether acetate: mass of bisphenol A diglycidyl ether = 1:1, and the amount of catalyst triphenylphosphine added for ring-opening reaction is 0.8wt% of the bisphenol A diglycidyl ether;

[0146] (2) cooling the chain-extended epoxy resin solution obtained in step (1) to 60° C., then adding acrylic acid, a ring-opening reaction catalyst triphenylphosphine and a polymerization inhibitor hydroquinone, and mixing, continuing to stir and react at 110° C. for 10 hours until the acid value of the reaction solution is less than 3 mgKOH / g, adjusting the temperature to 80° C., adding a polymerization inhibitor hydroquinone and tetrahydrophthalic anhydride, and mixing, and then adjusting the temperature to 100° C. and stirring and reacting for 6 hours to prepare a high-performance photosensitive epoxy resin;

[0147] The amount of triphenylphosphine as a catalyst for the ring-opening reaction is 0.8 wt % of the bisphenol A diglycidyl ether in step (1).

[0148] The amount of the polymerization inhibitor hydroquinone added each time is 0.4 wt % of the small molecular bisphenol epoxy compound in step (1).

[0149] Synthesis example 6

[0150] Synthesis Example 6 is to prepare a high-performance photosensitive epoxy resin based on chain extension modification of a small molecular bisphenol epoxy compound, and its raw materials mainly include, by mole:

[0151]

[0152] The diamine chain extender modifier is 1,3-bis(4'-aminophenoxy)benzene.

[0153] The preparation method of the high-performance photosensitive epoxy resin comprises the following steps:

[0154] (1) In an air atmosphere, preheat the solvent diethylene glycol ethyl ether acetate to 80° C., add bisphenol A diglycidyl ether and dissolve it, cool it to 60° C., add a diamine chain extender modifier, then heat it to 90° C., add triphenylphosphine as a catalyst for the ring-opening reaction, maintain the temperature at 90° C., and stir the reaction for 6 hours to obtain a chain-extended epoxy resin solution;

[0155] The mass of solvent diethylene glycol ethyl ether acetate: mass of bisphenol A diglycidyl ether = 1:1, and the amount of catalyst triphenylphosphine added for ring-opening reaction is 0.8wt% of the bisphenol A diglycidyl ether;

[0156] (2) cooling the chain-extended epoxy resin solution obtained in step (1) to 60° C., then adding acrylic acid, a ring-opening reaction catalyst triphenylphosphine and a polymerization inhibitor hydroquinone, and mixing, continuing to stir and react at 110° C. for 10 hours until the acid value of the reaction solution is less than 3 mgKOH / g, adjusting the temperature to 80° C., adding a polymerization inhibitor hydroquinone and tetrahydrophthalic anhydride, and mixing, and then adjusting the temperature to 100° C. and stirring and reacting for 6 hours to prepare a high-performance photosensitive epoxy resin;

[0157] The amount of triphenylphosphine as a catalyst for the ring-opening reaction is 0.8 wt % of the bisphenol A diglycidyl ether in step (1).

[0158] The amount of the polymerization inhibitor hydroquinone added each time is 0.4 wt % of the small molecular bisphenol epoxy compound in step (1).

[0159] Synthesis Example 7

[0160] In Synthesis Example 7, p-phenylenediamine is used as a diamine chain extender modifier, and the rest is consistent with the implementation method of Synthesis Example 1 to prepare a high-performance photosensitive epoxy resin.

[0161] Comparative Synthesis Example 1

[0162] Comparative Synthesis Example 1 is a photosensitive epoxy resin prepared by using a small molecular bisphenol epoxy compound but without chain extension modification. The raw materials thereof mainly include, by mole, the following:

[0163] 60 parts of bisphenol A diglycidyl ether,

[0164] 120 parts of acrylic acid,

[0165] 60 parts of tetrahydrophthalic anhydride.

[0166] The preparation method of the photosensitive epoxy resin comprises the following steps:

[0167] In an air atmosphere, preheat the solvent diethylene glycol ethyl ether acetate to 80°C, add bisphenol A diglycidyl ether and dissolve it, cool it to 60°C, then add acrylic acid, triphenylphosphine as a catalyst for ring-opening reaction and hydroquinone as a polymerization inhibitor, continue to stir and react at 110°C for 10 hours, until the acid value of the reaction solution is less than 3 mgKOH / g, adjust the temperature to 80°C, add hydroquinone as a polymerization inhibitor and tetrahydrophthalic anhydride, adjust the temperature to 100°C, stir and react for 6 hours, and prepare a photosensitive epoxy resin, denoted as BA;

[0168] The amount of triphenylphosphine as a catalyst for the ring-opening reaction is 0.8 wt % of the bisphenol A diglycidyl ether in step (1).

[0169] The amount of the polymerization inhibitor hydroquinone added each time is 0.4 wt % of the small molecular bisphenol epoxy compound in step (1).

[0170] Example 1

[0171] Example 1 is to use the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 1 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0172] 100 parts of high performance photosensitive epoxy resin,

[0173] Photoinitiator (ITX) 3 parts;

[0174] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0175] Example 2

[0176] Example 2 is to use the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 2 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0177] 100 parts of high performance photosensitive epoxy resin,

[0178] Photoinitiator (ITX) 3 parts;

[0179] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0180] Example 3

[0181] Example 3 is to use the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 3 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0182] 100 parts of high performance photosensitive epoxy resin,

[0183] Photoinitiator (ITX) 3 parts;

[0184] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0185] Example 4

[0186] Example 4 is to use the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 4 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0187] 100 parts of high performance photosensitive epoxy resin,

[0188] Photoinitiator (ITX) 3 parts;

[0189] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0190] Example 5

[0191] Example 5 is to use the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 5 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0192] 100 parts of high performance photosensitive epoxy resin,

[0193] Photoinitiator (ITX) 3 parts;

[0194] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0195] Example 6

[0196] Example 6 uses the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 6 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0197] 100 parts of high performance photosensitive epoxy resin,

[0198] Photoinitiator (ITX) 3 parts;

[0199] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0200] Example 7

[0201] Example 7 uses the high-performance photosensitive epoxy resin prepared in the above-mentioned Synthesis Example 7 as the main component to prepare a high-performance photosensitive solder resist ink, and its raw materials mainly include, by weight:

[0202] 100 parts of high performance photosensitive epoxy resin,

[0203] Photoinitiator (ITX) 3 parts;

[0204] After the components are preliminarily mixed in a blender, they are kneaded in a planetary ball mill to obtain the high-performance photosensitive solder resist ink.

[0205] However, the inventors found that when para-phenylenediamine was used as a diamine chain extender modifier, the mechanical properties of the ink finally prepared were significantly deteriorated. After horizontal experimental comparison, when the diamine chain extender modifier was selected except 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 1,3-bis(4'-aminophenoxy)benzene, and 1,4-butanediol bis(3-aminopropyl) ether, the mechanical properties all showed varying degrees of deterioration.

[0206] Comparative Example 1

[0207] Comparative Example 1 is to prepare a photosensitive solder resist ink using the photosensitive epoxy resin prepared in the above-mentioned synthetic comparative example 1 as the main component, and its raw materials mainly include, by weight:

[0208] 100 parts of photosensitive epoxy resin,

[0209] Photoinitiator (ITX) 3 parts;

[0210] The components are preliminarily mixed in a blender and then kneaded in a planetary ball mill to obtain the photosensitive solder resist ink.

[0211] When testing the high-performance photosensitive solder resist ink prepared in the above Examples 1 to 6 and the photosensitive solder resist ink prepared in Comparative Example 1, they were coated on a substrate, dried appropriately (about 75° C.), exposed to ultraviolet light for 60 seconds, and then heat treated at 150° C. for 60 minutes for further thermal curing, and naturally cooled to room temperature as samples.

[0212] 2. Test methods

[0213] Nuclear magnetic resonance spectroscopy (NMR) was measured using a Bruker ARX 600 NMR spectrometer from the United States using dimethyl sulfoxide-d 6 (DMSO-d 6 ) is a solvent.

[0214] Dynamic mechanical thermal analyzer (DMTA, TA Instruments Q850) was used to perform stress-strain curve and glass transition temperature tests in tensile mode. Stress-strain curve measurement: The sample was balanced at 25°C and 0.1N preload, and the load force was increased at a rate of 0.2N / min. In addition, in tensile mode and 0.01N preload, the sample was subjected to a 5°C / min -1 The tensile velocity is used to measure the stability of the sample as it changes with temperature.

[0215] Using German Concept-50 (Novocontrol) equipment in 1 2 -10 6 The broadband dielectric constant is measured at room temperature in the Hz frequency range. The diameter of the test sample is 20mm; the thickness is 0.05~0.1mm.

[0216] The DC voltage breakdown strength of the cured sample was recorded using a breakdown voltage tester with a rated voltage upper limit of 100 kV (Beijing Guance Precision Instrument Equipment). The size of the test sample was 20 mm × 20 mm; the thickness was 0.05 to 0.1 mm.

[0217] 3. Test results

[0218] Test results such as Figures 1 to 6 shown.

[0219] Among them, the high-performance photosensitive solder resist inks prepared in Examples 1 to 4 are compared as shown in Table 1 below:

[0220] Table 1

[0221]

[0222] It can be clearly seen that when the diamine chain extender modifier is 1,3-bis(4'-aminophenoxy)benzene, the overall dynamic thermomechanical properties of the cured specimens obtained are significantly better than those of Examples 1, 2 and 4; among them, the stress-strain performance under the tensile test conditions is surprising and much better than other options. The results of the example confirm that the main structure of 1,3-bis(4'-aminophenoxy)benzene Compared with 4,4'-diaminodiphenylmethane 4,4'-Diaminodiphenyl ether and 1,4-butanediol bis(3-aminopropyl) ether In terms of thermal properties, it has a more positive effect on improving the thermal and mechanical properties of bisphenol A type small molecule epoxy resin system.

[0223] Based on the above diamine chain extender modifier, 1,3-bis(4'-aminophenoxy)benzene is selected as the optimal solution. In Examples 3, 5, and 6, the molar ratio of the diamine chain extender modifier to acrylic acid is used as a variable to prepare the obtained high-performance photosensitive solder resist ink. The mechanical properties of the samples are compared as shown in Table 2 below:

[0224] Table 2

[0225]

[0226] It is obvious that in Examples 3, 5, and 6, as the molar ratio of the diamine chain extender modifier to acrylic acid gradually increases, the storage modulus (MPa), loss modulus (MPa), tensile stress (MPa), tensile strain (%), and toughness values ​​all show a significant trend of first increasing and then decreasing, but the tan (δ) value first decreases and then increases. When the molar ratio of 1,3-bis (4'-aminophenoxy) benzene to acrylic acid is 1:9 (Example 3), from the tensile stress-strain results, its overall thermal performance is better than the molar ratio in other embodiments, but from the perspective of dynamic thermomechanical properties, the Tg value under this formula is lower than that of Example 5 and Example 7, but the difference is within 3.6°C. The high-performance photosensitive epoxy resin obtained under this molar ratio has potential promotion and application value in the research and development of high-quality solder mask inks.

Claims

1. A high-performance photosensitive epoxy resin based on chain extension modification of small molecular bisphenol epoxy compounds, characterized in that The raw materials mainly include: 60 parts of small molecule bisphenol epoxy compounds, 3~22 parts of diamine chain extender modifier, Acrylic modifier 76~114 parts, 38-57 parts of acid anhydride, Among them, 2 times the molar fraction of the diamine chain extender modifier plus the molar fraction of the acrylic modifier totals 120 parts; The small molecule bisphenol epoxy compound is bisphenol A diglycidyl ether or bisphenol F diglycidyl ether; The diamine chain extender modifier is selected from any one of p-phenylenediamine, 4,4'-diaminobiphenyl, 2,2'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4''-diamino-p-terphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,3-propylenediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,4-butanediol bis(3-aminopropyl) ether, ethylene glycol bis(3-aminopropyl) ether, and bis(3-aminopropyl) ether; The high-performance photosensitive epoxy resin is obtained by firstly carrying out a chain extension reaction between a small molecular bisphenol epoxy compound and a diamine chain extension modifier, then carrying out a ring opening reaction with an acrylic modifier, and finally carrying out an esterification reaction with an acid anhydride.

2. The high performance photosensitive epoxy resin according to claim 1, characterized in that: The acrylic modifier is selected from at least one of acrylic acid, 2-furan acrylic acid, 2-thiophene acrylic acid, 3-(3-pyridyl) acrylic acid, 2-acetamido acrylic acid, 4-imidazole acrylic acid, terephthalic acid, trans-3-indole acrylic acid, 2-fluoroacrylic acid, and 2-benzyl acrylic acid.

3. The high performance photosensitive epoxy resin according to claim 1, characterized in that The method for preparing the high-performance photosensitive epoxy resin based on chain extension modification of small molecular bisphenol epoxy compounds mainly comprises the following steps: (1) In an air atmosphere, preheat the solvent to 75-95°C, add a small molecular bisphenol epoxy compound and dissolve it, cool it to 55-65°C, add a diamine chain extender modifier, then heat it to 75-95°C, add a catalyst for the ring-opening reaction, and then adjust the temperature to 85-95°C. Stir and react for 4-6 hours until the acid value of the reaction solution is less than 3 mgKOH / g, thereby obtaining a chain-extended epoxy resin solution; (2) The chain-extended epoxy resin solution obtained in step (1) is cooled to 55-65° C., and then an acrylic modifier, a catalyst for a ring-opening reaction and a polymerization inhibitor are added and mixed. The mixture is stirred and reacted at 100-110° C. for 8-12 hours until the acid value of the reaction solution is less than 3 mgKOH / g. The temperature is adjusted to 70-90° C., and a polymerization inhibitor and anhydride are added and mixed. The temperature is then adjusted to 95-105° C. and stirred and reacted for 6-8 hours to prepare a high-performance photosensitive epoxy resin.

4. The high performance photosensitive epoxy resin according to claim 3, characterized in that: The solvent in step (1) is at least one of a divalent acid ester high boiling point environmentally friendly solvent, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, dipropylene glycol methyl ether, propylene glycol methyl ether, trimethylbenzene and tetramethylbenzene; in step (1), the mass of the solvent: the mass of the small molecule bisphenol epoxy compound = (0.5~1.5):

1.

5. The high performance photosensitive epoxy resin according to claim 3, characterized in that: The polymerization inhibitor in step (2) is at least one of hydroquinone, o-methyl hydroquinone, p-hydroxyanisole, p-benzoquinone and 2,6-di-tert-butyl-4-methylphenol; the amount of the polymerization inhibitor added each time is 0.4-1.5wt% of the small molecular bisphenol epoxy compound in step (1).

6. The high performance photosensitive epoxy resin according to claim 3, characterized in that: The catalyst for the ring-opening reaction in step (2) is selected from any one of triethylamine, triethanolamine, 4-dimethylaminopyridine, tetrabutylammonium bromide, tetramethylammonium chloride, N,N-dimethylbenzylamine and triphenylphosphine; the amount of the catalyst added for the ring-opening reaction is 0.2-1 wt% of the small molecule bisphenol epoxy compound in step (1).

7. A high-performance photosensitive solder resist ink using the high-performance photosensitive epoxy resin of claim 1 as a main component, characterized in that The raw materials mainly include: 100 parts of high performance photosensitive epoxy resin, 2~5 parts of photoinitiator.

8. A high-performance photosensitive solder resist ink using the high-performance photosensitive epoxy resin of claim 1 as a main component, characterized in that The raw materials mainly include: 100 parts of high performance photosensitive epoxy resin, 2~5 parts of photoinitiator, 25~45 parts of filler, Additives 1~20 parts.

Citation Information

Patent Citations

  • A high-toughness, weakly alkaline water-developable photosensitive epoxy acrylate resin composition and its preparation method

    CN107450269B

  • Alcohol amine chain extender, and preparation method and applications thereof

    CN110862336A

  • A resin composition

    CN111607194A

  • Method for preparing high-performance photosensitive solder resist ink from naphthalene type chain extension modified epoxy resin

    CN116768728A

  • Nitrogen-containing epoxy resins for photocurable coating applications

    WO1998049214A1