A soft, skin-friendly, tear-resistant conductive silicone and preparation method thereof

By applying a soft and skin-friendly tear-resistant conductive silicone film on the clothing, the foreign body feeling and damage caused by conductive wires in the clothing is solved, the comfort and conductive properties of the clothing are improved, and the stable pulse massage feeling is provided.

CN117844253BActive Publication Date: 2024-12-03GUANGDONG QIYUE FUTURE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311587861.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-25
Publication Date
2024-12-03
Estimated Expiration
2043-11-25

AI Technical Summary

Technical Problem

The conductive wires that install pulsed parts in clothing are easily entangled in a mess, creating a foreign body feeling when worn, and are easily damaged during cleaning, reducing the comfort of the clothing.

Method used

Using soft and skin-friendly tear-resistant conductive silicone, the combination of components A and B forms a conductive silicone film and is applied to clothing to provide flexibility, tear-resistant and conductive, replacing conductive wires and avoiding Contact with the skin and provide a pulsed massage feeling when worn.

Benefits of technology

It improves the comfort of clothing, avoids wear and tear and fall off caused by long-term contact between the conductive silicone film and the human body, ensures the stability of conductive properties, provides a real massage feeling, and avoids the messy winding and damage of conductive wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117844253B_ABST
    Figure CN117844253B_ABST
Patent Text Reader

Abstract

The present application relates to the field of conductive silicone, and more specifically, it relates to a soft, skin-friendly, tear-resistant conductive silicone and a preparation method thereof. It comprises component A and component B in a mass ratio of (1-2): 1, wherein the component A comprises the following raw materials in parts by weight: 50-100 parts of vinyl-terminated silicone oil, 10-30 parts of methyl silicone oil, 2-10 parts of hydrogen-containing silicone oil, 10-30 parts of white carbon black, 20-100 parts of solvent, and 0.01-0.03 parts of platinum catalyst; component B is prepared from the following raw materials in parts by weight: 30-50 parts of conductive filler, 50-100 parts of solvent, and 0.01-0.2 parts of inhibitor. The conductive silicone film formed by the conductive silicone of the present application can be stably attached to the fabric to play a conductive role, and at the same time has the advantages of softness, skin-friendliness, and crack resistance. When used on clothing, it reduces the foreign body sensation and improves the comfort of clothing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of conductive silicone, and more specifically, to a soft, skin-friendly, tear-resistant conductive silicone and a preparation method thereof. Background Art

[0002] Clothing is a product that is sewn and worn on the human body for protection and decoration, or refers to various coverings made of cloth (such as cotton, silk, velvet, chemical fiber polyester, etc.) used by humans or through humans to cover the body.

[0003] Usually, in order to expand the functions of clothing, various functional accessories are set in the clothing to make it have other functions or roles. For example, massage beads are set inside the bra to play a massage role. However, the massage effect of this setting is not obvious. It can only play a massage role during exercise. For this reason, some people propose to install pulse and other components inside the bra.

[0004] Pulse usually refers to a pulse-like short-term undulating electrical shock (voltage or current) often used in electronic technology. The main characteristics are waveform, amplitude, width and repetition frequency. Pulse is a signal that occurs in a short time within the entire signal cycle relative to the continuous signal, and there is no signal in most signal cycles. Just like a human pulse, it can massage the corresponding acupuncture points of the human body.

[0005] When pulse components are installed inside the bra in clothing, the chest can be pulse treated or massaged. However, the conductive wires used for pulses are easily entangled when installed inside the bra, and when worn, the human chest has a foreign body sensation. At the same time, during the process of washing the bra, the conductive wires are easily folded, entangled or damaged, reducing the comfort of wearing the bra. Summary of the invention

[0006] In order to avoid the foreign body sensation when wearing clothes, maintain a better massage effect, and improve wearing comfort, the present application provides a soft, skin-friendly, tear-resistant conductive silicone and a preparation method thereof.

[0007] In a first aspect, the present application provides a soft, skin-friendly, tear-resistant conductive silicone rubber, comprising a component A and a component B in a mass ratio of (1-2):1, wherein the component A comprises the following raw materials in parts by weight:

[0008] 50-100 parts of vinyl terminated silicone oil

[0009] Methyl silicone oil 10-30 parts

[0010] 2-10 parts of hydrogen silicone oil

[0011] 10-30 parts of white carbon black

[0012] Solvent 20-100 parts

[0013] 0.01-0.03 parts of platinum catalyst;

[0014] Component B is prepared from the following raw materials in parts by weight:

[0015] Conductive filler 30-50 parts

[0016] Solvent 50-100 parts

[0017] Inhibitor 0.01-0.2 parts.

[0018] In the above scheme, the conductive silicone formed by the two combinations is used in clothing, which can have better softness, tear resistance and conductivity, avoid the use of conductive wires to touch the skin, and improve the comfort of the contact between the underwear and the human body.

[0019] Specifically, the side chain of terminal vinyl silicone oil has an active vinyl group, which is mainly used to prepare addition-type liquid silicone rubber base, and forms a polymer under the action of methyl silicone oil, hydrogen-containing silicone oil and catalyst, while white carbon black plays a filling role to improve its physical properties.

[0020] The conductive filler in component B not only plays a conductive role, but also plays a filling role, enhancing the physical properties of conductive silicone such as tear resistance. The solvents in components A and B can both play a diluting role, which makes it easier for the raw material system of conductive silicone to be fully mixed and evenly mixed, and also makes it easier for conductive silicone to be coated on clothing fabrics to form a conductive silicone film.

[0021] The conductive silicone film is soft and comfortable, has good conductivity and tear resistance, avoids contact with the human body and does not hurt the skin. It can be directly applied to any area of ​​​​the clothes by coating. After electricity is passed through, it can transmit current and make the coated area have a pulse massage feeling.

[0022] For example, Figure 1 As shown, conductive silicone is coated on the lower support part and the lower bowl part of the bra, and after curing, a conductive silicone film is formed, so that the conductive silicone film can transmit microcurrent, so that it has a pulse effect. Therefore, when the bra is worn, the corresponding chest position also has a pulse effect, and the conductive silicone film can be soft and skin-friendly to avoid the human body from having a foreign body sensation. At the same time, when the bra is washed, it is not easy to fall off, tear, or clump, thereby improving the comfort of wearing the bra.

[0023] The technical difficulties overcome or advantages possessed by the technology of this application are as follows: 1. The conductive silicone film formed by coating on clothing fabrics can stably adhere to the clothing fabrics; 2. The conductive silicone raw material system used still has better softness, better tear resistance and better conductivity even if thermal conductive fillers are added; 3. While ensuring the conductive performance, the conductive silicone film is prevented from being worn, falling off, agglomerated, etc. after long-term contact with the human body; 4. The conductive silicone film formed by the coating is in direct contact with the human body, and after being energized, the pulses generated make the massage feel more real and comfortable; 5. The power is supplied by a microcurrent, which will not cause harm to the human body; 6. The conductive silicone film is continuously connected to avoid the phenomenon of current interruption.

[0024] Preferably, the conductive filler is a modified conductive filler, and the modified conductive filler is composed of the following raw materials in parts by weight:

[0025] Polyol 20-30 parts

[0026] Isocyanate 5-15 parts

[0027] Compatibilizer 5-10 parts

[0028] Other additives 3-5 parts

[0029] 50-100 parts of carbon nanotubes.

[0030] In the above scheme, polyol is used as the raw material of polyurethane, and after reacting with isocyanate, the polyurethane composite formed has good softness, tear resistance, etc., and the compatibilizer can not only improve the compatibility of carbon nanotubes and polyurethane composites, but also improve the compatibility of polyurethane composites and conductive silicone raw material systems. Therefore, the present application further modifies carbon nanotubes by mixing polyol, isocyanate, compatibilizer, and other additives to obtain a composite, so that the modified carbon nanotubes obtained are easily dispersed in the conductive silicone raw material system, further improving the softness, tear resistance, conductivity and adhesion stability of the conductive silicone film formed by the conductive silicone on clothing, which can play a better pulse effect on the human body, and at the same time, improve the comfort of wearing clothing. Avoid, during use, it is placed on the skin.

[0031] Preferably, the polyol is one or more of methoxy polyethylene glycol polytrimethylene carbonate, bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol, and propylene oxide condensate.

[0032] After methoxy polyethylene glycol polytrimethylene carbonate, bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol, and propylene oxide condensate are polymerized, the obtained polyurethanes have good softness and tear resistance, etc. When the present application adopts multiple composites, they can play a synergistic role, further improve the tear resistance, and obtain better softness and adhesion.

[0033] Furthermore, each portion of the other additives consists of a plasticizer, a defoamer and a wetting agent in a weight ratio of (1-3): (1-2): 1.

[0034] With the assistance of the above plasticizers, defoamers and wetting agents, the conductive silicone can be further easily coated, and bubbles are not easily generated during the coating or processing process.

[0035] Preferably, the polyol is composed of polybutylene adipate glycol and polytrimethylene ether glycol in a weight ratio of 1:(1-3); or is composed of polybutylene adipate glycol and propylene oxide condensate in a weight ratio of 1:(1-2).

[0036] The above-mentioned polyester polyols and polyether polyols can be formed comprehensively, and after polymerization, the obtained polyurethane has good flexibility, tear resistance, adhesion and compatibility with conductive fillers. The modified conductive filler obtained is easy to be integrated into the raw material system of conductive silicone, and the softness, skin-friendliness, tear strength and stable adhesion of the conductive silicone film made of conductive silicone are further improved. When it is used in clothing and replaces the conductive wires of pulse and other components, it can reduce the foreign body sensation in the chest and improve the comfort of wearing clothing.

[0037] Preferably, the polyol is composed of three or more of methoxy polyethylene glycol polytrimethylene carbonate, bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol, and propylene oxide condensate.

[0038] Preferably, the polyol is composed of polybutylene adipate diol, polytrimethylene ether glycol, and methoxy polyethylene glycol polytrimethylene carbonate in a weight ratio of (1-2): (1-3): 1, or polybutylene adipate diol, polytrimethylene ether glycol, and bio-based modified castor oil polyol in a weight ratio of (1-3): (1-2): 1; or polybutylene adipate diol, polytrimethylene ether glycol, and bio-based modified castor oil polyol in a weight ratio of (1-3): (1-2): 1. The invention relates to a novel polyol comprising castor oil polyol and methoxy polyethylene glycol polytrimethylene carbonate in a weight ratio of (1-3): (1-2): (0.5-1.5): 1; or a polyol comprising methoxy polyethylene glycol polytrimethylene carbonate, bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol and propylene oxide condensate in a weight ratio of 1: (1-2): (1-2): (1-3): (1.5-2.5).

[0039] When the present invention is compounded by three kinds of polyols, the raw materials produce a synergistic effect, further improving its adhesion and tear resistance, while maintaining better softness and skin-friendliness.

[0040] Preferably, the compatibilizer is one or more of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, distearyloxyisopropoxyaluminate, trimethylolpropane triglycidyl ether, and ethylene-vinyl acetate copolymer.

[0041] The above-mentioned compatibilizers can further improve the compatibility of the conductive filler with the polyurethane composite, and also further improve the compatibility of the polyurethane composite with component A. Therefore, the prepared modified filler is easily compatible with the conductive silicone, and the obtained conductive silicone film has a stable structure, reduces the occurrence of tearing and cracking, and can stably adhere to the clothing fabric. At the same time, it is softer and skin-friendly, thereby improving the comfort of wearing clothing.

[0042] Preferably, the compatibilizer is composed of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, and ethylene-vinyl acetate copolymer in a weight ratio of 1:(1-3):(1-2).

[0043] Preferably, the compatibilizer is composed of diethylaminomethyltriethoxysilane, trimethylolpropane triglycidyl ether, and ethylene-vinyl acetate copolymer in a weight ratio of 1:(1-3):(1-2).

[0044] Preferably, the compatibilizer is composed of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, distearyloxyisopropoxyaluminate, trimethylolpropane triglycidyl ether, and ethylene-vinyl acetate copolymer in a weight ratio of 1:(1-3):(1-2):(1-2):(1-2).

[0045] Preferably, the compatibilizer is composed of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, distearyloxyisopropoxyaluminate, and ethylene-vinyl acetate copolymer in a weight ratio of 1:(1-3):(1-2):(1-2).

[0046] When the above-mentioned multiple compatibilizers are used for compounding, a synergistic effect can be achieved to further improve the compatibility of the modified conductive filler and the conductive silicone raw material system, thereby further improving the crack resistance, adhesion, softness and skin-friendliness of the conductive silicone film obtained.

[0047] The conductive filler is preferably straight carbon nanotubes, and has good electrical conductivity and thermal conductivity. Therefore, it is used in the raw material system of conductive silicone to achieve better conductive performance.

[0048] Preferably, the modified thermally conductive filler is prepared by the following method:

[0049] Weigh the polyol and other additives, mix them evenly, heat them to 100-120°C, and vacuum dehydrate them for 1-3 hours; cool them to 60-80°C, stir them at 20-30r / min for 20-30min, raise the temperature to 80-90°C, add isocyanate and compatibilizer, stir them evenly, then heat them to 100-120°C, react them in vacuum for 1-3 hours, cool them to 60-70°C, add carbon nanotubes, mix them evenly, and obtain a modified thermal conductive filler.

[0050] In the above production process, after the polyol is mixed with other additives, the moisture is removed by vacuuming, and the isocyanate and the compatibilizer are further reacted in one step to obtain a large molecular polyurethane material, and carbon nanotubes are further added to make them fully mixed with the polyurethane material. The modified thermal conductive filler thus obtained is used in conductive silicone to further improve the crack resistance, adhesion, softness and skin-friendliness of the conductive silicone film obtained.

[0051] In a second aspect, the present application provides a method for preparing soft, skin-friendly, tear-resistant conductive silicone, comprising the following steps:

[0052] Component A: Weigh vinyl-terminated silicone oil, methyl silicone oil, hydrogen-containing silicone oil, white carbon black, solvent, and platinum catalyst in parts by weight, and stir evenly to obtain component A;

[0053] Component B: According to parts by weight, weigh the conductive filler, solvent, and inhibitor and mix them evenly to obtain component B;

[0054] Component A and component B are mixed evenly in a weight ratio of (1-2):1 to obtain tear-resistant conductive silicone.

[0055] The above production process is simple to operate and has high production efficiency. The obtained conductive silicone is easy to be coated on the surface of clothing, and the conductive silicone film obtained by curing has good crack resistance, adhesion, softness and skin-friendliness, etc. When the clothing is made, it has good comfort during wearing.

[0056] In summary, this application has the following beneficial effects:

[0057] 1. Since the present application adopts component A formed by terminal vinyl silicone oil, methyl silicone oil, hydrogen-containing silicone oil, white carbon black, solvent, and platinum catalyst, and component B formed by conductive filler, solvent, and inhibitor, and mixes them in a ratio of (1-2):1 to obtain conductive silicone, it is easy to be coated on clothing fabrics and stably adhere to clothing fabrics. The conductive silicone film formed after curing has better tear resistance and softness. When it is used in clothing and worn, it avoids the feeling of foreign body and improves wearing comfort.

[0058] 2. The present application further modifies carbon nanotubes by mixing a composite obtained by mixing polyol, isocyanate, compatibilizer and other additives, so that the modified carbon nanotubes are easily dispersed in the conductive silicone raw material system, further improving the softness, tear resistance, conductivity and adhesion stability of the conductive silicone film formed by the conductive silicone on clothing, which can play a better pulse effect on the human body and improve the comfort of wearing clothing. Avoid touching the skin during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 The present invention discloses a bra picture containing a conductive silicone film. DETAILED DESCRIPTION

[0060] The following is combined with Figure 1 The present application is further described in detail with reference to the accompanying drawings and embodiments.

[0061] Some sources of raw materials or specific substances in the examples;

[0062] The isocyanate is hexamethylene diisocyanate;

[0063] The average molecular weight of methoxy polyethylene glycol polytrimethylene carbonate is 1000-2000;

[0064] The preferred manufacturer of bio-based modified castor oil polyol is Guangzhou Haoyi New Materials Technology Co., Ltd., model JT-805; the average molecular weight of polybutylene adipate diol is 1000-2000

[0065] The average molecular weight of polytrimethylene ether glycol is 1000-2000;

[0066] The propylene oxide condensate is poly(1,4-butylene adipate diol) with an average molecular weight of 1000 and a hydroxyl value of 106-118 mgKOH / g;

[0067] The vinyl-terminated silicone oil is a double-terminated vinyl silicone oil, with a vinyl content of 0.05-0.1% and a viscosity of 2000-20000 mPa·s;

[0068] The viscosity of methyl silicone oil is 500-1000mPa·s;

[0069] The hydrogen content of hydrogen-containing silicone oil is 0.10-0.5%;

[0070] The solvent is ethyl acetate;

[0071] The platinum content of the platinum catalyst is 20-40%;

[0072] The inhibitor is 1-ethynylcyclohexanol;

[0073] White carbon black mesh 300 mesh

[0074] The particle size of carbon nanotubes is 10-20nm;

[0075] The vinyl acetate (VA) content in the ethylene-vinyl acetate copolymer is 20% to 25%, and the average molecular weight is 20,000 to 30,000; the plasticizer is dibutyl phthalate;

[0076] The defoaming agent is Dow Corning AFE-3168 defoaming agent;

[0077] The leveling agent is manufactured by German BYK Chemical Co., Ltd., model: BYK-350.

[0078] Example

[0079] Example 1

[0080] A method for preparing soft, skin-friendly, tear-resistant conductive silicone comprises the following steps:

[0081] Component A: weigh 5kg of vinyl-terminated silicone oil, 1kg of methyl silicone oil, 0.2kg of hydrogen-containing silicone oil, 1kg of white carbon black, 5kg of solvent, and 0.001kg of platinum catalyst, mix them, and stir them at a speed of 40r / min for 30min to make them evenly stirred to obtain component A; Component B: weigh 3kg of conductive filler, 5kg of solvent, and 0.001kg of inhibitor, mix them, and stir them at a speed of 40r / min for 30min to make them evenly stirred to obtain component B;

[0082] 15 kg of component A and 10 kg of component B were mixed and stirred at a rotation speed of 40 r / min for 30 min to obtain tear-resistant conductive silicone.

[0083] Example 2-3

[0084] The difference between Example 2-3 and Example 1 is that the amount of raw materials used is different, as shown in Table 1;

[0085] Amount of raw materials used in Examples 1-5 (kg)

[0086]

[0087] Example 4

[0088] The difference between Example 4 and Example 2 is that the conductive filler is a modified conductive filler, which is prepared by the following method:

[0089] Weigh 2kg of polyol and 0.3kg of other additives, mix them evenly, heat them to 100℃, and perform vacuum dehydration for 3h at a vacuum degree of -0.1Mpa; cool them to 60℃, stir them at 20r / min for 30min, raise the temperature to 80℃, add 0.5kg of isocyanate and 0.5kg of compatibilizer, continue stirring for 20min, then heat to 100℃, perform vacuum reaction for 3h at a vacuum degree of -0.1Mpa, cool them to 60℃, add 5kg of carbon nanotubes, continue stirring for 30min, and obtain a modified thermal conductive filler.

[0090] The polyol is composed of polybutylene adipate glycol and polytrimethylene ether glycol in a weight (kg) ratio of 1:2;

[0091] The compatibilizer is diethylaminomethyltriethoxysilane.

[0092] Embodiment 5-6

[0093] The difference between Example 5-6 and Example 4 is that the amount of raw materials used is different and the process parameters are different, as shown in Table 2;

[0094] Table 2 Raw material dosage (kg) and process parameters of Examples 4-6

[0095]

[0096] Example 7

[0097] The difference between Example 7 and Example 5 is that the polyol is composed of polybutylene adipate diol and propylene oxide condensate in a weight (kg) ratio of 1:2.

[0098] Example 8

[0099] The difference between Example 8 and Example 5 is that the polyol is composed of polybutylene adipate glycol, polytrimethylene ether glycol, and methoxy polyethylene glycol polytrimethylene carbonate in a weight (kg) ratio of 2:3:1.

[0100] Example 9

[0101] The difference between Example 9 and Example 5 is that the polyol is composed of polybutylene adipate diol, polytrimethylene ether glycol, and bio-based modified castor oil polyol in a weight ratio of 2:2:1.

[0102] Example 10

[0103] The difference between Example 10 and Example 5 is that the polyol is composed of polybutylene adipate diol, polytrimethylene ether diol, bio-based modified castor oil polyol, and methoxy polyethylene glycol polytrimethylene carbonate in a weight (kg) ratio of 2:1:1:1.

[0104] Embodiment 11

[0105] The difference between Example 11 and Example 5 is that the polyol is composed of methoxy polyethylene glycol polytrimethylene carbonate, bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol, and propylene oxide condensate in a weight (kg) ratio of 1:1:2:3:2.

[0106] Example 12

[0107] The difference between Example 12 and Example 10 is that the compatibilizer is composed of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, and ethylene-vinyl acetate copolymer in a weight (kg) ratio of 1:3:2.

[0108] Embodiment 13

[0109] The difference between Example 13 and Example 11 is that the compatibilizer is composed of diethylaminomethyltriethoxysilane, trimethylolpropane triglycidyl ether, and ethylene-vinyl acetate copolymer in a weight (kg) ratio of 1:2:1.

[0110] Embodiment 14

[0111] The difference between Example 14 and Example 11 is that the compatibilizer is composed of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, distearyloxyisopropoxyaluminate, trimethylolpropane triglycidyl ether, and ethylene-vinyl acetate copolymer in a weight (kg) ratio of 1:2:1:2:1.

[0112] Embodiment 15

[0113] The difference between Example 15 and Example 11 is that the compatibilizer is composed of diethylaminomethyltriethoxysilane, bis(dioctylpyrophosphate)ethylene titanate, distearyloxyisopropoxyaluminate, and ethylene-vinyl acetate copolymer in a weight (kg) ratio of 1:2:2:1.

[0114] Performance testing

[0115] Detection method / test method

[0116] The conductive silicone obtained in Example 1-15 was coated on the fabric (Modal polyester fabric, specifications: composition and content: Modal 72%, polyester 28%, yarn count 40*40, density 150*90, gram weight 108g / ㎡), and cured at 120°C for 30 minutes to form a 100μm conductive silicone film.

[0117] 1. Tear resistance

[0118] The conductive silicone obtained in Examples 1-15 was coated on a release film and cured at 120° C. for 30 minutes. The 100 μm conductive silicone film was peeled off to obtain a test sample. The tear strength of the conductive silicone film was tested according to ASTM D624, and the average value was obtained by measuring 3 times.

[0119] 2. Peel strength

[0120] The fabric containing the conductive silicone film is cut into 1 inch*1 inch test samples. Test: Refer to GB / T2791(2)-1995 standard to test the peel strength, and measure 3 times to get the average value.

[0121] 3. Softness

[0122] The conductive silicone obtained in Example 1-15 was placed in a mold, heated to 130° C., and cured for 1 hour to obtain a 3 cm conductive silicone block. The hardness was then tested with reference to GB / T531-1999 standard, and the average value was taken after three measurements.

[0123] The above experimental data are shown in 3;

[0124] Table 3 Experimental data of Examples 1-15

[0125]

[0126]

[0127] Combining Example 1 and Example 4 and Table 3, it can be seen that the tear resistance and peel strength of Example 1 are lower than those of Example 4, while the hardness is slightly reduced. This shows that when modified conductive fillers are used, the conductive silicone film made of conductive silicone can have better tear resistance, adhesion and softness. Therefore, when used in clothing, it reduces discomfort caused by contact with the skin and reduces the possibility of the conductive silicone film falling off during use.

[0128] Combining Example 4 with Examples 8-11, it can be seen that the tear resistance and peel strength of Examples 8-11 are higher than those of Example 4, indicating that when three or more polyols are used for compounding, a synergistic effect can be achieved, further enabling the conductive silicone film made of conductive silicone to have both better tear resistance and adhesion. In addition, the hardness of Examples 8-11 is not much different from that of Example 4, indicating that the present application obtains better tear resistance and adhesion while maintaining better softness and skin-friendliness.

[0129] Combining Example 10 with Examples 12-15, it can be seen that the tear resistance and peel strength of Examples 12-15 are higher than those of Example 10, and the hardness is lower than that of Example 10, indicating that after compounding with a variety of compatibilizers, the modified conductive filler obtained is more easily compatible with the raw material system of conductive silicone, thereby obtaining better tear resistance, adhesion, skin-friendly softness, etc.

[0130] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A soft, skin-friendly, tear-resistant conductive silicone, characterized in that: The invention comprises component A and component B in a mass ratio of (1-2): 1, wherein component A is composed of the following raw materials in parts by weight: 50-100 parts of vinyl terminated silicone oil Methyl silicone oil 10-30 parts 2-10 parts of hydrogen silicone oil 10-30 parts of white carbon black Solvent 20-100 parts 0.01-0.03 parts of platinum catalyst; Component B is prepared from the following raw materials in parts by weight: Conductive filler 30-50 parts Solvent 50-100 parts Inhibitor 0.01-0.2 parts; The conductive filler is a modified conductive filler, and the modified conductive filler is composed of the following raw materials in parts by weight: Polyol 20-30 parts Isocyanate 5-15 parts Compatibilizer 5-10 parts Other additives 3-5 parts 50-100 parts of carbon nanotubes; Each portion of the other additives is composed of a plasticizer, a defoamer and a wetting agent in a weight ratio of (1-3): (1-2): 1; The polyol is one or more of bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol, and propylene oxide condensate; The compatibilizer is composed of two or more of diethylaminomethyltriethoxysilane, bis(dioctyloxypyrophosphate)ethylene titanate, distearyloxyisopropoxyaluminate, and trimethylolpropane triglycidyl ether; The modified conductive filler is prepared by the following method: Weigh the polyol and other additives, mix them evenly, heat them to 100-120°C, and vacuum dehydrate them for 1-3h; cool them to 60-80°C, stir them at 20-30r / min for 20-30min, raise the temperature to 80-90°C, add isocyanate and compatibilizer, stir them evenly, heat them to 100-120°C, react them in vacuum for 1-3h, cool them to 60-70°C, add carbon nanotubes, mix them evenly, and obtain a modified conductive filler; The preparation method of the tear-resistant conductive silica gel comprises the following steps: Component A: Weigh vinyl-terminated silicone oil, methyl silicone oil, hydrogen-containing silicone oil, white carbon black, solvent, and platinum catalyst in parts by weight, and stir evenly to obtain component A; Component B: According to parts by weight, weigh the conductive filler, solvent, and inhibitor and mix them evenly to obtain component B; Component A and component B are mixed evenly in a weight ratio of (1-2):1 to obtain tear-resistant conductive silicone.

2. The soft, skin-friendly, tear-resistant conductive silicone according to claim 1, characterized in that: The polyol is composed of polybutylene adipate glycol and polytrimethylene ether glycol in a weight ratio of 1:(1-3); or is composed of polybutylene adipate glycol and propylene oxide condensate in a weight ratio of 1:(1-2).

3. The soft, skin-friendly, tear-resistant conductive silicone according to claim 1, characterized in that: The polyol is composed of three or more of bio-based modified castor oil polyol, polybutylene adipate glycol, polytrimethylene ether glycol, and propylene oxide condensate.