Fe3o4 magnetic nanoclusters with high light-heat conversion efficiency for photothermal tumor treatment, preparation method and application thereof

By synthesizing and heat-treating Fe3O4 magnetic nanoclusters using a solvothermal method, the problem of low photothermal conversion efficiency of existing Fe3O4 nanomaterials was solved, enabling efficient photothermal therapy for tumors and reducing treatment side effects.

CN117860884BActive Publication Date: 2026-11-10DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410027378.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-09
Publication Date
2026-11-10
Estimated Expiration
2044-01-09

AI Technical Summary

Technical Problem

Existing Fe3O4 nanomaterials exhibit poor photothermal properties under near-infrared light and low photothermal conversion efficiency, leading to the need for more materials and higher laser power during treatment, which can easily cause side effects. Existing methods for improving these properties are complex and lack universality.

Method used

Fe3O4 magnetic nanoclusters were synthesized by a solvothermal method and then heat-treated at high temperature to increase grain size and material defect density, thereby improving electron nonradiative relaxation rate and photothermal conversion efficiency.

Benefits of technology

Fe3O4 magnetic nanoclusters with high photothermal conversion efficiency were prepared, which significantly improved the photothermal performance of the material, reduced the side effects of treatment, and achieved safe and efficient photothermal therapy for tumors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117860884B_ABST
    Figure CN117860884B_ABST
Patent Text Reader

Abstract

A kind of high light-heat conversion efficiency type Fe3O4 magnetic nanocluster for tumor photothermal therapy, preparation method and application thereof belong to the technical field of tumor photothermal therapy.The magnetic nanocluster is synthesized by surface stabilizer trisodium citrate, and the precursor is prepared by small crystal grain aggregation, and then the precursor is prepared by heat treatment;The magnetic nanocluster is spinel ferrite, has large Fe3O4 crystal grain size and high material defect density, and has high light-heat conversion efficiency.FeCl3, Na3Cit·2H2O, NaAc and EG are uniformly mixed to form a solution, then transferred to hydrothermal kettle for solvothermal reaction to generate precursor magnetic nanocluster, and then the final high light-heat conversion efficiency magnetic nanocluster is formed by later heat treatment, and the light-heat conversion efficiency of the magnetic nanocluster can reach more than 50%.The preparation method is economical and simple, easy to popularize, the prepared magnetic nanocluster is spinel structure ferrite with stable chemical properties, has excellent light-heat conversion efficiency, and improves the safety of photothermal therapy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of tumor photothermal therapy technology, and relates to magnetic media for photothermal therapy, and in particular to a high photothermal conversion efficiency Fe3O4 magnetic nanoclusters for tumor photothermal therapy and their applications. Background Technology

[0002] Malignant tumors (cancer), as a disease characterized by the uncontrolled growth of abnormal cells, have a high incidence and mortality rate, making them one of the world's largest public health problems. Currently, the main treatments for cancer include surgery, chemotherapy, and radiation therapy. However, surgery is typically targeted at patients in the early stages of cancer, and the removal of tumor tissue inevitably involves the removal of some normal tissue, easily leading to sequelae and functional impairment. While chemotherapy and radiation therapy can effectively kill spreading tumor cells, their severe toxic side effects can cause significant damage to the patient's body.

[0003] Studies have shown that tumor cells are more sensitive to temperature than normal cells. Based on temperature range, hyperthermia can be divided into traditional hyperthermia (42–46℃) and high-temperature hyperthermia (46–60℃). Photothermal therapy utilizes the property of photothermal media to heat up under near-infrared light. The photothermal media is implanted or introduced into the tumor tissue area, and then near-infrared light is irradiated to raise its temperature, thereby inhibiting or killing tumor cells. Compared to surgical treatment, chemotherapy, and radiotherapy, photothermal therapy has the advantages of low toxicity and minimal damage, making it a safe and environmentally friendly treatment method.

[0004] Fe3O4 nanomaterials possess stable crystal structures, are easily degradable, have low preparation costs, and exhibit excellent magnetic properties. They have also been approved for clinical use by the US Food and Drug Administration (FDA) as a T2-weighted contrast agent in magnetic resonance imaging (MRI), thus making them widely applicable in the biological field. However, nano-Fe3O4 exhibits poor photothermal performance under near-infrared light, with a photothermal conversion efficiency generally below 25%. This necessitates higher material injection doses and laser power in treatments, potentially leading to side effects. Current methods to improve photothermal performance mainly include enhancing magnetic coupling by self-assembling individual Fe3O4 particles into superstructures to increase the probability of ligand field transitions; coating Fe3O4 with special organic materials such as indocyanine dye IR806 and polypyrrole to inject additional electrons provided by the organic materials under near-infrared light into the Fe3O4 band structure to induce ligand-metal charge transfer transitions; and modifying the Fe3O4 synthesis method to alter the crystal orientation. Based on these methods, the photothermal conversion efficiency of nano Fe3O4 is currently the highest, reaching only 42%. In addition, the complexity of the synthesis process and the weak universality are also drawbacks of these methods.

[0005] To address the issue of generally low photothermal conversion efficiency in reported Fe3O4 nanomaterials, this invention starts from the essence of photothermal conversion, namely the conversion of electron energy during electron relaxation. By applying high temperatures to the material, a large number of electron traps are introduced into the electronic band structure, thereby increasing the non-radiative relaxation speed of electrons and converting light energy into heat energy more effectively. Ultimately, a high photothermal conversion efficiency Fe3O4 magnetic nanoclusters are prepared for tumor photothermal therapy. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing high-photothermal-conversion-efficiency Fe3O4 magnetic nanoclusters for photothermal therapy and its application. The method utilizes a solvothermal approach to synthesize precursor Fe3O4 magnetic nanoclusters composed of small crystallites using trisodium citrate as a surface stabilizer. This precursor is then transferred to a tube furnace for heat treatment to generate the final Fe3O4 magnetic nanoclusters. The magnetic nanoclusters prepared by this invention are spinel ferrites, chemically stable, and characterized by high photothermal conversion efficiency, making them suitable for tumor photothermal therapy. This method is economical, convenient, and easy to promote.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A high-efficiency photothermal conversion Fe3O4 magnetic nanoclusters for tumor photothermal therapy are disclosed. Compared with previously reported magnetic nanoclusters, these nanoclusters possess larger Fe3O4 grain sizes and higher material defect densities. Conventional solvothermal methods for forming magnetic nanoclusters require the introduction of surface stabilizers, but the addition of these stabilizers restricts grain growth, limiting grain size to extremely small levels. Furthermore, the reaction temperatures required for conventional solvothermal methods are generally low, resulting in low material defect densities. This invention primarily addresses these two issues by introducing heat treatment. After heat treatment, based on the Oswald ripening mechanism, the grain size can be significantly increased, thereby enhancing magnetic coupling and improving photothermal conversion efficiency. Additionally, the high temperature after heat treatment creates more defects in the clusters, increasing electron traps in the band structure and enabling rapid nonradiative relaxation of electrons to convert energy into heat, further improving photothermal conversion efficiency.

[0009] The photothermal conversion efficiency of the Fe3O4 magnetic nanoclusters can reach over 50%.

[0010] The Fe3O4 magnetic nanoclusters have large Fe3O4 grain sizes ranging from 13.0 nm to 15.0 nm.

[0011] An application of a high-efficiency photothermal conversion magnetic nanoclusters for tumor photothermal therapy is disclosed, which enables effective tumor treatment. The magnetic nanoclusters are mixed with physiological saline to prepare a stable suspension, which is then injected into the tumor area. The tumor area is irradiated with near-infrared light of appropriate power density, and the magnetic nanoclusters rapidly convert light energy into heat energy, raising the tumor temperature to the target temperature. After short-term, multiple-cycle treatments, tumor growth can be effectively inhibited and tumor volume reduced.

[0012] A method for preparing magnetic nanoclusters for high photothermal conversion efficiency tumor photothermal therapy includes the following steps:

[0013] Step 1: Prepare mixed solution A

[0014] Anhydrous ferric chloride and trisodium citrate dihydrate were placed in ethylene glycol and magnetically stirred at 500–800 rpm for 1–3 hours at 20–40 °C until completely dissolved, preparing a mixed solution A with a molar ratio of ferric chloride, trisodium citrate, and ethylene glycol of 1:0.05–1:30–200. Ferric chloride provides Fe for the solvothermal reaction. 3+ Ethylene glycol has both the properties of a solvent and a reducing agent for Fe. 3+ The role of trisodium citrate as a surface stabilizer is to promote the aggregation of crystal grains into clusters. It is particularly important to emphasize that trisodium citrate, rather than commonly used polymers (such as PAA, PEG, PEI, etc.), was chosen as the surface stabilizer to ensure high saturation magnetization and reduce high-temperature carbonization.

[0015] The second step is to prepare mixed solution B.

[0016] Anhydrous sodium acetate is placed in mixed solution A and magnetically stirred at 500-800 r / min for 0.5-2 h at 20-40℃ until completely dissolved, thus preparing mixed solution B with a molar ratio of ferric chloride, trisodium citrate, sodium acetate, and ethylene glycol of 1:0.05-1:0.5-20:30-200 (preferably 1:0.1-0.4:1-8:50-120). Sodium acetate provides an alkaline environment for the solvothermal reaction.

[0017] The third step involves a solvothermal reaction to generate the precursor Fe3O4 magnetic nanoclusters.

[0018] The mixed solution B was transferred to a hydrothermal reactor and sealed, with the volume ratio of mixed solution B to the volume of the hydrothermal reactor being 1:2.5. The hydrothermal reactor was placed in a drying oven and heated at 200–250°C for 5–12 hours, and then allowed to cool naturally to room temperature to obtain a magnetic suspension.

[0019] Step 4: Cleaning and drying

[0020] The obtained magnetic suspension was repeatedly washed with deionized water and anhydrous ethanol alternately. Each time, the suspension was first ultrasonically dispersed for 5–10 minutes, then placed on a magnet for 5–20 minutes. Afterward, the upper layer of suspension was poured off under the magnet's attraction, and then deionized water or anhydrous ethanol was added and ultrasonically dispersed again. This cycle was repeated 5–10 times, ending with washing with deionized water. The precipitate obtained after washing was then placed in a vacuum freezer and dried at -80 to -40°C for 24–48 hours to obtain magnetic powder, which was then finely ground using a grinding rod.

[0021] Step 5, heat treatment

[0022] The powder obtained in step four is placed in a tube furnace and heated at a rate of 1–20 °C / min (preferably 8–12 °C / min) under argon, nitrogen, or helium protection, and held at 250–800 °C (preferably 300–500 °C) for 0.5–5 h (preferably 1–3 h). It is then allowed to cool naturally to room temperature, with the protective gas flow rate set to 100–200 sccm. The resulting powder is then finely ground using a grinding rod to obtain the final Fe3O4 magnetic nanoclusters, which are stored at 0–4 °C. This process is based on the synthesized clusters, utilizing high-temperature heating to promote grain growth and introduce more defects.

[0023] In this invention, Fe 3+ The amounts of ion-derived ferric chloride and the surface stabilizer trisodium citrate directly affect the grain size and structural stability of the product. Insufficient ferric chloride (excessive trisodium citrate) may result in excessively small grain size, leading to weak magnetic coupling and low photothermal conversion efficiency. Conversely, excessive ferric chloride (insufficient trisodium citrate) may leave some grains unprotected by the surface stabilizer, resulting in poor product structural stability and unsuitability for practical applications.

[0024] Heat treatment temperature and time directly affect the grain size, defect density, and surface functional groups of the product. Heat treatment of the prepared magnetic nanoclusters increases grain size while simultaneously increasing defects such as lattice disorder, thermal disturbance, and oxygen vacancies. This enhances magnetic coupling and introduces more electron traps into the band structure to promote rapid nonradiative relaxation of electrons, thereby improving photothermal conversion efficiency. Higher heat treatment temperatures and longer heat treatment times may lead to larger grain sizes and defect densities, resulting in higher photothermal conversion efficiency. However, higher heat treatment temperatures and longer heat treatment times may also weaken surface functional groups, causing more significant aggregation, increasing scattering in aqueous solutions, and reducing photothermal conversion efficiency.

[0025] The heating rate during heat treatment directly affects the uniformity of the product's size and shape. An excessively rapid heating rate results in uneven grain heating and inconsistent growth, which is detrimental to size and shape uniformity. While an excessively slow heating rate is beneficial for size and shape uniformity, it increases unnecessary time costs.

[0026] Effects and benefits of the present invention:

[0027] This invention proposes a method for preparing magnetic nanoclusters with high photothermal conversion efficiency for tumor photothermal therapy and their applications. These clusters not only possess a chemically stable spinel structure and inherent magnetic properties, but also exhibit excellent photothermal conversion efficiency, significantly improving the photothermal performance of the material. This ensures that the desired therapeutic effect can still be achieved using small doses of magnetic nanoclusters and low-power lasers, greatly reducing potential side effects during treatment and further improving treatment safety. Furthermore, the preparation method is economical, simple, and easy to promote. Attached Figure Description

[0028] Figure 1 This is a flowchart of the sample preparation process of the present invention;

[0029] Figure 2 These are transmission electron microscope images of the samples, where (a) is the sample of the present invention and (b) is the untreated sample;

[0030] Figure 3 These are the X-ray diffraction patterns of the samples, where (a) is the sample of the present invention and (b) is the untreated sample;

[0031] Figure 4 This is the extinction performance curve of the sample of this invention;

[0032] Figure 5 These are the temperature rise and fall curves and photothermal conversion efficiency of the samples based on near-infrared light, where (a) is the sample of the present invention and (b) is the untreated sample.

[0033] Figure 6 These are the Urbach energy results for the samples, where (a) is the sample of the present invention and (b) is the untreated sample. Detailed Implementation

[0034] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0035] The following will combine the technical implementation scheme and the accompanying drawings. Figure 2 , Figure 3 , Figure 4 , Figure 5 and Figure 6 The specific embodiments of the present invention will be described in detail. Figure 2(a) is a transmission electron microscope image of the Fe3O4 magnetic nanoclusters prepared in Example 1, which shows that they have a cluster structure composed of grains. Figure 3 (a) is the X-ray diffraction pattern of the Fe3O4 magnetic nanoclusters prepared in Example 1, which confirms its spinel structure, and the grain size can be calculated to be 14.0 nm using the Scherrer equation. Figure 4 The figure shows the extinction performance curve of the Fe3O4 magnetic nanoclusters prepared in Example 1. The wide range and high extinction in the figure indicate that the prepared clusters can effectively utilize near-infrared light, which is beneficial to improving the photothermal effect. Figure 5 (a) shows the heating curve of the Fe3O4 magnetic nanoclusters prepared in Example 1 under near-infrared light and the cooling curve after removing near-infrared light. It can be seen that the sample can heat up significantly and rapidly. The photothermal conversion efficiency can be calculated to be 51.1%.

[0036] According to the two Fe3O4 magnetic nanoclusters described in Example 1 and Comparative Example 1, such as Figure 2 As shown, after heat treatment, the grain size of the clusters increased significantly; as Figure 3 As shown, after heat treatment, the crystallinity of the cluster crystal structure increases, and the grain sizes for heat-treated and untreated structures can be calculated using the Scherrer equation to be 14.0 nm and 7.3 nm, respectively, indicating a significant increase in grain size; Figure 5 As shown, after heat treatment, the photothermal properties of the clusters were significantly enhanced, with the photothermal conversion efficiency increasing from 31.6% to 51.1%; Figure 6 As shown, after heat treatment, the Urbach energy of the clusters increased significantly from 0.461 eV to 0.692 eV. The Urbach energy represents defects in the material caused by lattice disorder, thermal disturbance, oxygen vacancies, etc.; the higher the defect density, the higher the Urbach energy. According to Examples 1, 2, and 3, the three Fe3O4 magnetic nanoclusters all exhibited significant temperature increases under near-infrared light, with photothermal conversion efficiencies all exceeding 50%.

[0037] In summary, these results demonstrate that the Fe3O4 magnetic nanoclusters prepared in this invention possess excellent photothermal conversion efficiency and photothermal performance. Specific examples are as follows:

[0038] Example 1

[0039] 1) Preparation of mixed solution A: Add 2.8g of anhydrous ferric chloride and 1.0g of trisodium citrate dihydrate to 80mL of ethylene glycol, and stir magnetically at 600r / min for 2h at 30℃ to ensure complete dissolution;

[0040] 2) Preparation of mixed solution B: Add 4.6g of anhydrous sodium acetate to the above solution and stir continuously at the same temperature and stirring rate for 1h to completely dissolve the sodium acetate.

[0041] 3) Solvent thermal reaction to generate precursor Fe3O4 magnetic nanoclusters: The mixed solution B was transferred to a 200mL hydrothermal reactor and sealed. The hydrothermal reactor was then placed in a drying oven and heated at 220℃ for 10h. After that, it was naturally cooled to room temperature to obtain a magnetic suspension.

[0042] 4) Washing and Drying: The obtained magnetic suspension was repeatedly washed with deionized water and anhydrous ethanol alternately. Each time, the suspension was first ultrasonically dispersed for 8 minutes, then placed on a magnet for 10 minutes. Afterward, the upper layer of suspension was poured off under the magnet's attraction, and then deionized water or anhydrous ethanol was added and ultrasonically dispersed again. This cycle was repeated 8 times, ending with washing with deionized water. The precipitate obtained after washing was then placed in a vacuum freezer and dried at -60°C for 36 hours to obtain magnetic powder, which was then finely ground using a grinding rod.

[0043] 5) Heat treatment: The powder obtained in step 4) was placed in a tube furnace and heated at 400℃ for 2 hours under the protection of argon gas at a flow rate of 150 sccm, with a heating rate of 10℃ / min. The powder was then allowed to cool naturally to room temperature. The resulting powder was then finely ground with a grinding rod to obtain the final Fe3O4 magnetic nanoclusters, which were stored in a refrigerator at 4℃.

[0044] The prepared magnetic nanoclusters were subjected to in vitro photothermal heating experiments to verify their photothermal performance and photothermal conversion efficiency. The specific steps of the in vitro photothermal heating experiment are as follows:

[0045] 1) Preparation of magnetic nanocluster suspension: Weigh 10 mg of magnetic nanocluster and add it to 50 mL of deionized water to prepare a magnetic nanocluster suspension of 0.2 mg / mL. Disperse the suspension by sonication for 10 min. After mixing evenly, extract 0.2 mL of the suspension and add it to a 1.5 mL conical centrifuge tube.

[0046] 2) Photothermal heating experiment: The centrifuge tube containing the suspension obtained in step 1) was placed in an atmosphere with a wavelength of 808 nm and a power density of 1 W / cm². 2 The sample was irradiated with near-infrared light for 10 minutes, followed by a 10-minute break. Temperature data were recorded every 30 seconds during the heating and cooling process using a thermal imager, and a heating and cooling curve over time was plotted.

[0047] In this embodiment, the photothermal conversion efficiency of the Fe3O4 magnetic nanoclusters is 51.1%. The large Fe3O4 grain size is 14.0 nm.

[0048] Comparative Example 1

[0049] 1) Preparation of mixed solution A: Add 2.8g of anhydrous ferric chloride and 1.0g of trisodium citrate dihydrate to 80mL of ethylene glycol, and stir magnetically at 600r / min for 2h at 30℃ to ensure complete dissolution;

[0050] 2) Preparation of mixed solution B: Add 4.6g of anhydrous sodium acetate to the above solution and stir continuously at the same temperature and stirring rate for 1h to completely dissolve the sodium acetate.

[0051] 3) Solvent thermal reaction to generate precursor Fe3O4 magnetic nanoclusters: The mixed solution B was transferred to a 200mL hydrothermal reactor and sealed. The hydrothermal reactor was then placed in a drying oven and heated at 220℃ for 10h. After that, it was naturally cooled to room temperature to obtain a magnetic suspension.

[0052] 4) Washing and Drying: The obtained magnetic suspension was repeatedly washed with deionized water and anhydrous ethanol alternately. Each time, the suspension was first ultrasonically dispersed for 8 minutes, then placed on a magnet for 10 minutes. The upper layer of suspension was then poured off under the magnet's attraction. Deionized water or anhydrous ethanol was then added, followed by ultrasonic dispersion. This cycle was repeated 8 times, ending with washing with deionized water. The precipitate obtained after washing was then placed in a vacuum freezer and dried at -60°C for 36 hours. It was then finely ground with a grinding rod to obtain the final Fe3O4 magnetic nanoclusters, which were stored at 4°C.

[0053] The prepared magnetic nanoclusters were subjected to photothermal heating experiments in vitro to verify their photothermal performance and photothermal conversion efficiency, as detailed in Example 1.

[0054] Example 2

[0055] 1) Preparation of mixed solution A: Add 2.0 g of anhydrous ferric chloride and 0.35 g of trisodium citrate dihydrate to 80 mL of ethylene glycol, and stir magnetically at 800 r / min for 3 h at 20 °C to ensure complete dissolution;

[0056] 2) Preparation of mixed solution B: Add 7.8g of anhydrous sodium acetate to the above solution and stir continuously at the same temperature and stirring rate for 0.5h to completely dissolve the sodium acetate.

[0057] 3) Solvent thermal reaction to generate precursor Fe3O4 magnetic nanoclusters: The mixed solution B was transferred to a 200mL hydrothermal reactor and sealed. The hydrothermal reactor was then placed in a drying oven and heated at 200℃ for 12h. After that, it was naturally cooled to room temperature to obtain a magnetic suspension.

[0058] 4) Washing and Drying: The obtained magnetic suspension was repeatedly washed with deionized water and anhydrous ethanol alternately. Each time, the suspension was first ultrasonically dispersed for 10 minutes, then placed on a magnet for 20 minutes. After that, the upper layer of suspension was poured off under the magnet's attraction, and then deionized water or anhydrous ethanol was added and ultrasonically dispersed again. This cycle was repeated 5 times, ending with washing with deionized water. The precipitate obtained after washing was then placed in a vacuum freezer and dried at -40°C for 48 hours to obtain magnetic powder, which was then finely ground using a grinding rod.

[0059] 5) Heat treatment: The powder obtained in step 4) was placed in a tube furnace and heated at a rate of 8°C / min under nitrogen protection at a flow rate of 100 sccm, and held at 500°C for 1 hour, then allowed to cool naturally to room temperature. The resulting powder was then finely ground with a grinding rod to obtain the final Fe3O4 magnetic nanoclusters, which were stored in a refrigerator at 4°C.

[0060] The prepared magnetic nanoclusters were subjected to photothermal heating experiments in vitro to verify their photothermal performance and photothermal conversion efficiency, as detailed in Example 1.

[0061] In this embodiment, the photothermal conversion efficiency of the Fe3O4 magnetic nanoclusters is 50.2%. The large Fe3O4 grain size is 14.9 nm.

[0062] Example 3

[0063] 1) Preparation of mixed solution A: Add 4.7g of anhydrous ferric chloride and 3.4g of trisodium citrate dihydrate to 80mL of ethylene glycol, and stir magnetically at 500r / min for 1h at 40℃ to ensure complete dissolution;

[0064] 2) Preparation of mixed solution B: Add 2.4g of anhydrous sodium acetate to the above solution and stir continuously for 2 hours at the same temperature and stirring rate to completely dissolve the sodium acetate.

[0065] 3) Solvent thermal reaction to generate precursor Fe3O4 magnetic nanoclusters: The mixed solution B was transferred to a 200mL hydrothermal reactor and sealed. The hydrothermal reactor was then placed in a drying oven and heated at 250℃ for 5h. After that, it was naturally cooled to room temperature to obtain a magnetic suspension.

[0066] 4) Washing and Drying: The obtained magnetic suspension was repeatedly washed with deionized water and anhydrous ethanol alternately. Each time, the suspension was first ultrasonically dispersed for 5 minutes, then placed on a magnet for 5 minutes. After that, the upper layer of suspension was poured off under the magnet's attraction, and then deionized water or anhydrous ethanol was added and ultrasonically dispersed again. This cycle was repeated 10 times, ending with washing with deionized water. The precipitate obtained after washing was then placed in a vacuum freezer and dried at -80°C for 24 hours to obtain magnetic powder, which was then finely ground using a grinding rod.

[0067] 5) Heat treatment: The powder obtained in step 4) was placed in a tube furnace and heated at 300℃ for 3 hours under the protection of helium at a flow rate of 200 sccm, with a heating rate of 12℃ / min. The powder was then allowed to cool naturally to room temperature. The resulting powder was then finely ground with a grinding rod to obtain the final Fe3O4 magnetic nanoclusters, which were stored in a 0℃ refrigerator.

[0068] The prepared magnetic nanoclusters were subjected to photothermal heating experiments in vitro to verify their photothermal performance and photothermal conversion efficiency, as detailed in Example 1.

[0069] In this embodiment, the photothermal conversion efficiency of the Fe3O4 magnetic nanoclusters is 50.6%. The large Fe3O4 grain size is 13.2 nm.

[0070] The above-described embodiments are merely illustrative of the implementation methods of the present invention, but should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the protection scope of the present invention.

Claims

1. A method for preparing Fe3O4 magnetic nanoclusters for high photothermal conversion efficiency tumor photothermal therapy, characterized in that, Includes the following steps: The first step is to prepare mixed solution A; Anhydrous ferric chloride and trisodium citrate dihydrate are placed in ethylene glycol and completely dissolved at 20-40°C to prepare a mixed solution A with a molar ratio of ferric chloride, trisodium citrate and ethylene glycol of 1:0.05-1:30-200. The second step is to prepare mixed solution B; Anhydrous sodium acetate is placed in mixed solution A and completely dissolved at a temperature of 20~40℃ to prepare mixed solution B with a molar ratio of ferric chloride, trisodium citrate, sodium acetate and ethylene glycol of 1: 0.1~0.4:1~8:50~120; The third step involves a solvothermal reaction to generate the precursor Fe3O4 magnetic nanoclusters. The mixed solution B was transferred to a hydrothermal reactor and sealed. The volume ratio of the mixed solution B to the volume of the hydrothermal reactor was 1:2.

5. The hydrothermal reactor was placed in a drying oven and heated at 200~250℃ for 5~12 h. After that, it was naturally cooled to room temperature to obtain a magnetic suspension. The fourth step is washing and drying; The obtained magnetic suspension was repeatedly washed with deionized water and anhydrous ethanol, and the precipitate was vacuum dried to obtain magnetic powder. Step 5: Heat treatment; The magnetic powder obtained in step four was finely ground and placed in a tube furnace. Under inert gas protection, the temperature was raised from room temperature to 300-500℃ and held for 1-3 hours, then naturally cooled to room temperature. The flow rate of the protective gas was set to 100-200 sccm. The obtained powder was finely ground with a grinding rod to obtain Fe3O4 magnetic nanoclusters, which were then stored at 0-4℃. The heating rate was 1-20℃ / min. The Fe3O4 magnetic nanoclusters are prepared by synthesizing a precursor composed of small crystallites using trisodium citrate as a surface stabilizer, followed by heat treatment of the precursor. The magnetic nanoclusters are spinel ferrites, possessing large Fe3O4 grain size and high material defect density, resulting in high photothermal conversion efficiency.

2. The method for preparing Fe3O4 magnetic nanoclusters for high photothermal conversion efficiency tumor photothermal therapy according to claim 1, characterized in that, The photothermal conversion efficiency can reach over 50%.

3. The method for preparing Fe3O4 magnetic nanoclusters for high photothermal conversion efficiency tumor photothermal therapy according to claim 1, characterized in that, The size range of the large Fe3O4 grains is 13.0 nm to 15.0 nm.

4. The method for preparing Fe3O4 magnetic nanoclusters for high photothermal conversion efficiency tumor photothermal therapy according to claim 1, characterized in that, In the fourth step, each time the suspension is cleaned, it must first be ultrasonically dispersed and then placed on a magnet. After 5 to 20 minutes, the upper layer of suspension is poured off under the attraction of the magnet. Then, deionized water or anhydrous ethanol is added and ultrasonically dispersed again. This cycle is repeated 5 to 10 times, ending with cleaning with deionized water. The vacuum drying temperature is -80 to -40°C, and the drying time is 24 to 48 hours.