A nitrocellulose membrane, its preparation method and application

By optimizing the interwoven fiber structure and node distribution of nitrocellulose membranes, the problems of high liquid flow resistance and membrane clogging were solved, enabling effective separation of large protein molecules and improved sensitivity of immunochromatography.

CN117861462BActive Publication Date: 2026-11-17HANGZHOU COBETTER FILTRATION EQUIPMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311742207.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2026-11-17
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

Existing nitrocellulose membranes are prone to forming nodal structures during liquid flow, resulting in high liquid flow resistance, affecting the flow of large protein molecules, easily clogging the membrane, and increasing background depth when colloidal gold is used as a colorimetric agent.

Method used

By controlling the interlacing structure of nitrocellulose fibers, adjusting the relationship between the number of nodes per unit area, the average diameter of nodes, and the average pore size on the outer surface, the fiber diameter and node distribution are optimized, reducing node formation and creating a more uniform pore structure.

Benefits of technology

It achieves efficient separation of large protein molecules at lower flow rates, reduces membrane clogging and background depth, and improves the sensitivity and uniformity of immunochromatography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117861462B_ABST
    Figure CN117861462B_ABST
Patent Text Reader

Abstract

This application relates to the field of protein chromatography technology, specifically to nitrocellulose membranes, their preparation methods, and applications. In this application, the nitrocellulose membrane is formed by nitrocellulose fibers, which interweave to form a network structure and create internal channels for liquid passage. The fibers have nodes, and on the outer surface, the number of nodes per unit area N1, the average node diameter R1, and the average SEM pore size D1 of the outer surface satisfy the following relationship: N1·R1 3 =D1·K1, where K1 ranges from 3% to 20%. The nitrocellulose membrane in this application has a low creep rate and small porosity, while exhibiting low non-specific adsorption of large protein molecules, reducing background color during use and improving uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of protein chromatography technology, specifically to nitrocellulose membranes and their preparation methods and applications. Background Technology

[0002] Chromatography is a commonly used method for the detection, separation, and purification of proteins. In chromatography, immunochromatography with a chromogenic reagent is a novel antigen detection technique. This technique uses a microporous membrane as a carrier, immobilizing specific antigens or antibodies on the carrier. The sample to be tested is placed at the other end, and capillary action forces the sample through the region containing the chromogenic reagent, where it is captured. The chromogenic reagent that binds to the antigenic components in the sample is then captured by the specific antigen or antibody targeting that antigen, ultimately accumulating on the detection line and forming a color. The chromogenic reagent that does not bind to the antigen fails to accumulate on the detection line and instead accumulates on the control line. This method is convenient, stable, intuitive, and low-cost, making it widely applicable.

[0003] In immunochromatography, in order to allow the target antigen or target antibody in the sample to react with the chromogenic agent or the specific antibody or antigen on the detection line, it is necessary to control the crawling speed of the liquid on the microporous membrane. The slower the crawling speed, the longer the reaction time. Generally, the crawling speed is related to the pore size of the microporous membrane; the smaller the pore size, the slower the crawling speed.

[0004] Nitrocellulose membranes are microporous filter membranes commonly used in immunochromatography. They possess advantages such as stability, weak non-specific adsorption, uniform overall structure, high strength, and resistance to dirt and folding, and are currently widely used in various test strips. Nitrocellulose membranes are typically prepared via a phase separation method. During this process, nitrocellulose precipitates out under non-solvent or vapor conditions, forming a microporous structure. However, in this process, after precipitation, nitrocellulose tends to adsorb onto its surface under kinetic effects, forming aggregated nodular structures. The distribution of these nodules causes meandering in the liquid flow channels, increasing the resistance to liquid flow in the chromatogram.

[0005] Colloidal gold is a typical chromogenic agent, known for its excellent colorimetric effect and typically small particle size. When microporous membranes have low porosity, small flow pore size, and low creep rate, using colloidal gold as a chromogenic agent allows it to pass smoothly through the microporous membrane, achieving higher sensitivity and lower background color. However, when the protein itself is large, the colloidal gold bound to the protein undergoes significant changes in volume and binding performance. Therefore, when the flow resistance caused by the cluster distribution in nitrocellulose membranes is high, it can easily impede the flow of colloidal gold particles adsorbed with the analyte protein, resulting in a large background depth. Summary of the Invention

[0006] In order to provide an immunochromatographic microporous membrane with low climbing speed, small porosity, and low non-specific adsorption of macromolecular proteins, this application provides a nitrocellulose membrane and a method for preparing the same.

[0007] The nitrocellulose membrane involved in this application is formed by nitrocellulose fibers. The fibers interweave to form a network structure, creating flow channels for liquid to pass through. The fibers have nodes. On the outer surface, the number of nodes per unit area N1, the average node diameter R1, and the average SEM pore size D1 of the outer surface satisfy the following relationship: N1·R1 3 =D1·K1, where K1 ranges from 3% to 20%.

[0008] In the aforementioned technical solution, during the separation of proteins with large molecular weights using nitrocellulose membranes at relatively low flow rates, the proteins increase in size after binding to antibodies, making them prone to becoming stuck in the membrane pores. This prevents subsequent large molecules from passing through, resulting in membrane blockage. Membrane blockage is typically related to the structure of the nitrocellulose membrane. During the preparation of the nitrocellulose membrane, nodules are formed on the fibers. These nodules are approximately spherical structures formed by the aggregation of some nitrocellulose fibers, thus significantly influencing the siphon effect within the membrane and the mechanical effects on the proteins. In this application, when filtering proteins with large molecular weights or irregular shapes, the number of nodules per unit area, the average diameter of the nodules, and the average pore size on the outer surface must satisfy the relationship shown in the formula above, where (N1·R1) 3 ) / D1 should be within a constant range, meaning that the range of selectable average pore diameters is proportional to the number of nodes and the cube of the node diameter. Under this condition, the larger the number of nodes and the larger the node diameter, the larger the overall porosity should be. Since the appearance of nodes will increase the specific surface area and increase the number of concave structures in the membrane, more protein enrichment is more likely to occur in the densely distributed nodes, and the membrane is more likely to be blocked. Therefore, the greater the distribution density of nodes, the smaller the required node diameter. At a larger porosity, the requirements of the above characteristics can be more lenient, but the creep rate is also more difficult to control.

[0009] Preferably, the value of K1 and the average diameter R2 of the fiber satisfy the following relationship: K1 = K2 · R2 2 Wherein, the value of K2 ranges from 0.6% to 3.0%.

[0010] Within a specific pore area ratio range, generally, the larger the fiber diameter, the larger the corresponding pore size. Overall, with a larger fiber diameter, the fiber spreads more smoothly, thus forming better flow channels to guide liquid flow. In the above scheme, the square of the fiber diameter is basically proportional to the value of K1; that is, the larger the fiber diameter, the greater the node density and the larger the node diameter can be accommodated under conditions of similar surface SEM average pore size.

[0011] Preferably, the average diameter R2 of the fiber is 2 to 3 μm; and the average diameter R1 of the node is 4 to 7 μm.

[0012] In the above scheme, the system should have relatively coarse fibers while maintaining a specific pore area ratio. In this state, the possibility of protein or protein bound to antibody being blocked by fibers is small, and the resulting pore structure is more regular. However, the fibers should not be too coarse, otherwise it will easily cause inhomogeneity within the system, leading to strip distortion. Based on the above, while maintaining the above-mentioned fiber diameter values, the system should not currently have a large average diameter of fiber knots. Otherwise, excessively large fiber knots will seriously affect the uniformity of the system, causing different capillary forces in different regions of the membrane, thereby reducing the smoothness of the scribing area.

[0013] Preferably, the number of nodes per unit area N1 and the average node diameter R1 have the following relationship: N1·R1 2 =K3; where K3 ranges from 0.1 to 0.26 μm, and the number of nodes per unit area N1 is no greater than 15 per (50 μm). 2

[0014] In this application, the number and size of the nodes should be inversely related; the larger the number of nodes, the smaller the required node size. Specifically, the number of nodes should be inversely proportional to the square of the node diameter. Since the nodes will block the alkalinity of the material in the cross-section of the membrane, K3, within a certain range, can reduce the influence of the nodes on the siphon effect and liquid flow resistance. However, the nodes cannot be too small and too dense; otherwise, excessively fine nodes will create regions with a large specific surface area inside the cellulose membrane. In these regions, the adsorption performance of the nitrocellulose membrane for proteins will be significantly enhanced. Therefore, a small and dense node arrangement should be avoided.

[0015] Preferably, the ratio of the average node diameter R1 on the outer surface to the average SEM aperture D1 on the outer surface is not greater than 0.66.

[0016] The average diameter of the nodes on the outer surface should be kept within a small range compared to the average pore size of the outer surface. That is, while maintaining a relatively large outer surface pore size, the average diameter of the nodes should be kept as small as possible, thereby reducing the unevenness of the fiber surface and improving the smoothness and uniformity of protein flow.

[0017] Preferably, the proportion P2 of the length of the nitrocellulose fiber covered by knots is 3-6.5% of the total length of the nitrocellulose fiber.

[0018] During liquid flow, nitrocellulose fibers can act as guides. As the liquid and protein move along the fibers, the nodes can change the flow direction and regulate the flow rate. However, excessively large or dense nodes can cause defects in the system, making it easier for proteins to get stuck, which leads to more frequent membrane blockage. Therefore, in the above scheme, the density of nodes on the fibers is limited. Under this condition, when the liquid flows with the fibers, the protein is less likely to be stuck by the nodes on the fibers, further reducing the occurrence of membrane blockage.

[0019] Preferably, on the nitrocellulose fiber, the ratio P2 of the length covered by the knot to the total length of the nitrocellulose fiber has the following relationship with the ratio P3 between the fiber diameter and the knot diameter: P2∶P3=6~12%.

[0020] In the above scheme, the more prominent the nodes are relative to the fiber diameter, the sparser their distribution density on the fiber should be. Otherwise, more indentations and grooves are easily generated on the fiber, making it easier for proteins to get stuck. Furthermore, nodes that are more prominent than the fiber, even with a denser node distribution, are also more likely to create numerous small gaps in the system, making them more prone to jamming. In the above formula, the proportion of the length covered by nodes to the total length of the nitrocellulose fiber is inversely proportional to the ratio between the node diameter and the fiber diameter, and their product should be within a specific range.

[0021] In addition, this application also relates to a method for preparing the above-mentioned nitrocellulose membrane, which includes the following steps:

[0022] S1. Prepare the casting solution, which includes 5-20 parts by weight of nitrocellulose, 80 parts of organic solvent, 5-20 parts of nonionic surfactant, and 0.1-10 parts of aliphatic polyol.

[0023] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film.

[0024] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film.

[0025] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0026] During the formation of nitrocellulose membranes, due to the inherent instability of nitrocellulose distribution in solution, its precipitation initially forms small spheres, which then connect with each other through fiber connections, resulting in an interwoven network structure. These spheres are the nodes described in this application. In this application, a low-concentration nitrocellulose molecular solution is prepared and pretreated through evaporation and phase separation, followed by solvent phase separation. During vacuum phase separation, the formation of new nodes is reduced, and a basic cross-linked structure is formed within the system. Subsequent phase separation further forms a network structure based on this initial cross-linking. In this state, large-volume nodes are less likely to form, and the overall number of nodes is also smaller.

[0027] Preferably, in step S2, the temperature is controlled at 15–30°C, the humidity at 30–50%, and the time at 1–60 seconds.

[0028] Experiments showed that controlling the temperature and vacuum level further reduced the formation of knots. Furthermore, the vacuum level allowed for better control of the nucleation process, resulting in more uniform fiber precipitation and the formation of a homogeneous nitrocellulose membrane. Simultaneously, maintaining low humidity within the system helped reduce the rate of polymer precipitation in this step.

[0029] Preferably, in step S3, the coagulation bath is a sodium chloride solution with a mass concentration of 0.1% to 1%.

[0030] In the above technical solution, the coagulation bath is set with a sodium chloride solution of a certain concentration. By adjusting the charge balance in the solution, the precipitation rate of nitrocellulose can be controlled, so that a more uniform and satisfactory nitrocellulose membrane can be formed.

[0031] Preferably, in step S3, the temperature is controlled at 10–30°C and the phase separation time is 20–600 s.

[0032] In the above scheme, using a lower temperature and a slower phase separation setting can effectively control the generation of new nodes. At a lower temperature, nitrocellulose molecules are more inclined to attach to existing fibers or extend on existing cores. At the same time, in order to form a lower energy system, a better cross-linking system will be generated rather than a system with more nodes, resulting in a membrane structure with obvious fibrosis and a small number of nodes.

[0033] Preferably, the aliphatic polyol is glycerol, and the glycerol has a mass fraction of 1 to 5 parts.

[0034] In the above system, the viscosity, spreading properties and product precipitation properties of the casting solution are adjusted by adding glycerol. Glycerol itself can be washed with water after processing, and it can also adjust the precipitation properties of nitrocellulose to achieve uniform precipitation.

[0035] This application also relates to the application of nitrocellulose membranes in the field of immunochromatography, which can be prepared into immunochromatographic test strips or kits for use in immunochromatography with chromogenic agents such as colloidal gold and latex microspheres.

[0036] In summary, this application designs and synthesizes a novel nitrocellulose membrane that can be used for the immunochromatographic detection of target proteins. With a low climbing rate and small pore size, it reduces the obstruction of colloidal gold particles adsorbed with target proteins in the chromatography, thereby reducing membrane clogging and lowering the background depth. Attached Figure Description

[0037] Figure 1 This is a SEM image of the nitrocellulose membrane surface in Example 1 of this application;

[0038] Figure 2 This is a SEM image of the nitrocellulose membrane surface in Example 10 of this application;

[0039] Figure 3 This is a schematic diagram of the homogeneity of nitrocellulose membrane chromatography in Example 1;

[0040] Figure 4 This is a schematic diagram of the homogeneity of nitrocellulose membrane chromatography in Example 6;

[0041] Figure 5 This is a schematic diagram of the uniformity of the nitrocellulose membrane scribing in Example 1;

[0042] Figure 6 This is a schematic diagram of the uniformity of the nitrocellulose membrane markings in Example 14. Detailed Implementation

[0043] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0044] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0045] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0046] The average pore size on the surface of nitrocellulose membranes, or the average pore size of the cross-section, or the number of nodes, can all be determined by characterizing the membrane structure using a scanning electron microscope (SEM), followed by measurement and calculation using computer software (such as Matlab, NIS-Elements, etc.) or manually. In actual measurement, the membrane surface can be characterized first using an electron microscope to obtain the corresponding SEM image. Since the pores on the membrane surface are roughly uniform, a certain area, such as 1 μm, can be selected. 2 (1μm x 1μm) or 25μm 2 (5μm x 5μm), the specific area size depends on the actual situation. Then, use the corresponding computer software or manually measure the diameter of all holes or nodes on this area, and then calculate to obtain the average hole diameter and the average diameter of nodes on this surface.

[0047] The areas of nodes and holes can be calculated in the same way. This can be done by manually dividing the approximate hole and node regions and then analyzing and calculating them using a computer, or by using a grid method. Similarly, fiber length can be calculated by manually marking the fiber trajectory and then using a computer.

[0048] It should be noted that those skilled in the art can also obtain the above parameters through other measurement methods, and the above measurement methods are for reference only.

[0049] Examples 1 through 30 all involve nitrocellulose membranes, and each example has different parameters, as shown in Table 1.

[0050] Table 1

[0051]

[0052]

[0053]

[0054] In Table 1, K1 = N1·R1 3 / D1, K2 = K1 / R2 2 K3 = N1·R1 2 .

[0055] The statistical method for determining node distribution density involves dividing the region, counting the number of nodes with clear outlines, and averaging the results across multiple 50μm*50μm squares. Some nodes are approximately circular, while others have irregular shapes. These irregularly shaped nodes are typically formed by the fusion of two or more closely spaced nuclei during node formation and are counted as a single node in the statistical analysis.

[0056] When calculating the average SEM pore size and pore area ratio of the membrane, only the pore size of the outermost pores under the SEM microscope is counted, i.e., the outermost ring formed by the fiber structure in the image. The fiber length and diameter are also only counted for the outermost fibers, i.e., those not obscured by other fibers. During the formation of the mesh structure, fibers will form... Figure 1 The intersection points shown in region A are not counted as nodes in this region, nor are their widths included in the fiber diameter statistics. When calculating fiber length, these intersection points are abstracted as points without area, and each point is connected to the others for fiber length calculation. In this process, whether a node covers part or all of the fiber, the calculation is based on the portion of the fiber covered by the node.

[0057] By adjusting different preparation methods, nitrocellulose membranes with different microstructures can be prepared. It should be noted that the following only provides methods for preparing the microstructures of the corresponding nitrocellulose membranes. Nitrocellulose membranes with the same microstructures prepared by other methods not described in the following examples should have similar effects and are also within the scope of protection of this application.

[0058] The preparation method of the nitrocellulose membrane in Example 1 is as follows:

[0059] S1. Prepare the casting solution, which by weight includes 10 parts nitrocellulose, 80 parts organic solvent, 10 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0060] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 45%, and the time is 30s.

[0061] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0062] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0063] The preparation method of the nitrocellulose membrane in Example 2 is as follows:

[0064] S1. Prepare the casting solution, which includes 15 parts nitrocellulose, 80 parts organic solvent, 4 parts Tween 60, and 0.1 parts glycerol by weight; the organic solvent is acetone.

[0065] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 30°C, the humidity is controlled at 50%, and the time is 30 seconds.

[0066] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.1%, the temperature is 25℃, and the processing time is 200s.

[0067] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0068] The preparation method of the nitrocellulose membrane in Example 3 is as follows:

[0069] S1. Prepare the casting solution, which by weight includes 12 parts nitrocellulose, 80 parts organic solvent, 10 parts Tween 60, and 5 parts glycerol; the organic solvent is acetone.

[0070] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 40%, and the time is 50 seconds.

[0071] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 30℃, and the processing time is 400s.

[0072] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0073] The preparation method of the nitrocellulose membrane in Example 4 is as follows:

[0074] S1. Prepare the casting solution, which by weight includes 6 parts nitrocellulose, 80 parts organic solvent, 8 parts Tween 60, and 5 parts glycerol; the organic solvent is acetone.

[0075] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 15℃, the humidity is controlled at 35%, and the time is 15s.

[0076] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.2%, the temperature is 30℃, and the processing time is 540s.

[0077] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0078] The preparation method of the nitrocellulose membrane in Example 5 is as follows:

[0079] S1. Prepare the casting solution, which by weight includes 8 parts nitrocellulose, 80 parts organic solvent, 6 parts lauryl alcohol polyoxyethylene ether, and 4.5 parts glycerin; the organic solvent is acetone.

[0080] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 20°C, the humidity is controlled at 40%, and the time is 45s.

[0081] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.2%, the temperature is 20℃, and the processing time is 540s.

[0082] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0083] The preparation method of the nitrocellulose membrane in Example 6 is as follows:

[0084] S1. Prepare the casting solution, which by weight includes 18 parts nitrocellulose, 80 parts organic solvent, 10 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0085] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 10℃, the humidity is controlled at 30%, and the time is 60s.

[0086] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.1%, the temperature is 30℃, and the processing time is 600s.

[0087] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0088] The preparation method of the nitrocellulose membrane in Example 7 is as follows:

[0089] S1. Prepare the casting solution, which by weight includes 15 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 1 part glycerol; the organic solvent is acetone.

[0090] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 40℃, the humidity is controlled at 60%, and the time is 20s.

[0091] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.8%, the temperature is 25℃, and the processing time is 240s.

[0092] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0093] The preparation method of the nitrocellulose membrane in Example 8 is as follows:

[0094] S1. Prepare the casting solution, which by weight includes 17 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 8 parts ethylene glycol; the organic solvent is acetone.

[0095] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 50%, and the time is 5s.

[0096] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 30℃, and the processing time is 90s.

[0097] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0098] The preparation method of the nitrocellulose membrane in Example 8 is as follows:

[0099] S1. Prepare the casting solution, which by weight includes 5 parts nitrocellulose, 80 parts organic solvent, 15 parts Tween 60, and 10 parts glycerol; the organic solvent is acetone.

[0100] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 15℃, the humidity is controlled at 50%, and the time is 5s.

[0101] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0102] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0103] The preparation method of the nitrocellulose membrane in Example 9 is as follows:

[0104] S1. Prepare the casting solution, which by weight includes 13 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 2.5 parts glycerol; the organic solvent is acetone.

[0105] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 45%, and the time is 30s.

[0106] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0107] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0108] The preparation method of the nitrocellulose membrane in Example 10 is as follows:

[0109] S1. Prepare the casting solution, which by weight includes 16 parts nitrocellulose, 80 parts organic solvent, 16 parts Tween 60, and 8 parts glycerol; the organic solvent is acetone.

[0110] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 35%, and the time is 20s.

[0111] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is pure water, the temperature is 25℃, and the processing time is 120s.

[0112] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0113] The preparation method of the nitrocellulose membrane in Example 11 is as follows:

[0114] S1. Prepare the casting solution, which by weight includes 18 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0115] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 35%, and the time is 50s.

[0116] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.3%, the temperature is 25℃, and the processing time is 600s.

[0117] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0118] The preparation method of the nitrocellulose membrane in Example 12 is as follows:

[0119] S1. Prepare the casting solution, which by weight includes 16 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 5 parts glycerol; the organic solvent is acetone.

[0120] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 30°C, the humidity is controlled at 30%, and the time is 45s.

[0121] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 600s.

[0122] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0123] The preparation method of the nitrocellulose membrane in Example 13 is as follows:

[0124] S1. Prepare the casting solution, which by weight includes 8 parts nitrocellulose, 80 parts organic solvent, 6 parts Tween 60, and 1 part glycerol; the organic solvent is acetone.

[0125] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 50%, and the time is 5s.

[0126] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.8%, the temperature is 30℃, and the processing time is 300s.

[0127] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0128] The preparation method of the nitrocellulose membrane in Example 14 is as follows:

[0129] S1. Prepare the casting solution, which by weight includes 30 parts nitrocellulose, 80 parts organic solvent, 15 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0130] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 50%, and the time is 60s.

[0131] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0132] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0133] The preparation method of the nitrocellulose membrane in Example 15 is as follows:

[0134] S1. Prepare the casting solution, which by weight includes 12 parts nitrocellulose, 80 parts organic solvent, 8 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0135] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 30°C, the humidity is controlled at 40%, and the time is 45s.

[0136] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0137] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0138] The preparation method of the nitrocellulose membrane in Example 16 is as follows:

[0139] S1. Prepare the casting solution, which by weight includes 15 parts nitrocellulose, 80 parts organic solvent, 15 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0140] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 20°C, the humidity is controlled at 30%, and the time is 60s.

[0141] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 30℃, and the processing time is 240s.

[0142] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0143] The preparation method of the nitrocellulose membrane in Example 17 is as follows:

[0144] S1. Prepare the casting solution, which by weight includes 15 parts nitrocellulose, 80 parts organic solvent, 12 parts Tween 60, and 1.5 parts glycerol; the organic solvent is acetone.

[0145] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 20°C, the humidity is controlled at 45%, and the time is 40s.

[0146] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 20℃, and the processing time is 180s.

[0147] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0148] The preparation method of the nitrocellulose membrane in Example 18 is as follows:

[0149] S1. Prepare the casting solution, which includes 6 parts by weight of nitrocellulose, 80 parts of organic solvent, 6 parts of Tween 60, and 1.5 parts of glycerol; the organic solvent is acetone.

[0150] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 50%, and the time is 30s.

[0151] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0152] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0153] The preparation method of the nitrocellulose membrane in Example 19 is as follows:

[0154] S1. Prepare the casting solution, which by weight includes 12 parts nitrocellulose, 80 parts organic solvent, 12 parts Tween 60, and 5 parts glycerol; the organic solvent is acetone.

[0155] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 20°C, the humidity is controlled at 40%, and the time is 40s.

[0156] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 240s.

[0157] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0158] The preparation method of the nitrocellulose membrane in Example 20 is as follows:

[0159] S1. Prepare the casting solution, which by weight includes 8 parts nitrocellulose, 80 parts organic solvent, 15 parts Tween 60, and 10 parts glycerol; the organic solvent is acetone.

[0160] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 50%, and the time is 30s.

[0161] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0162] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0163] The preparation method of the nitrocellulose membrane in Example 21 is as follows:

[0164] S1. Prepare the casting solution, which includes 18 parts by weight of nitrocellulose, 80 parts of organic solvent, 2 parts of Tween 60, and 0.5 parts of glycerol; the organic solvent is acetone.

[0165] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 50%, and the time is 60s.

[0166] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 20℃, and the processing time is 180s.

[0167] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0168] The preparation method of the nitrocellulose membrane in Example 22 is as follows:

[0169] S1. Prepare the casting solution, which by weight includes 10 parts nitrocellulose, 80 parts organic solvent, 25 parts Tween 60, and 10 parts glycerol; the organic solvent is acetone.

[0170] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 30%, and the time is 90s.

[0171] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 180s.

[0172] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0173] The preparation method of the nitrocellulose membrane in Example 23 is as follows:

[0174] S1. Prepare the casting solution, which by weight includes 5 parts nitrocellulose, 80 parts organic solvent, 15 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0175] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 45%, and the time is 120s.

[0176] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 20s.

[0177] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0178] The preparation method of the nitrocellulose membrane in Example 24 is as follows:

[0179] S1. Prepare the casting solution, which by weight includes 7 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 3 parts propylene glycol; the organic solvent is acetone.

[0180] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 30°C, the humidity is controlled at 45%, and the time is 60s.

[0181] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a 1% sodium chloride solution at a temperature of 30°C and a processing time of 60 seconds.

[0182] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0183] The preparation method of the nitrocellulose membrane in Example 25 is as follows:

[0184] S1. Prepare the casting solution, which by weight includes 6 parts nitrocellulose, 80 parts organic solvent, 6 parts Tween 60, and 2 parts glycerol; the organic solvent is acetone.

[0185] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 45%, and the time is 30s.

[0186] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 120s.

[0187] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0188] The preparation method of the nitrocellulose membrane in Example 26 is as follows:

[0189] S1. Prepare the casting solution, which by weight includes 12 parts cellulose nitrate, 80 parts organic solvent, 6 parts Tween 60, and 2 parts glycerol; the organic solvent is acetone.

[0190] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 15℃, the humidity is controlled at 45%, and the time is 60s.

[0191] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.1%, the temperature is 30℃, and the processing time is 50s.

[0192] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0193] The preparation method of the nitrocellulose membrane in Example 27 is as follows:

[0194] S1. Prepare the casting solution, which by weight includes 10 parts nitrocellulose, 80 parts organic solvent, 8 parts Tween 60, and 3 parts glycerol; the organic solvent is acetone.

[0195] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 20°C, the humidity is controlled at 45%, and the time is 45s.

[0196] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 20℃, and the processing time is 180s.

[0197] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0198] The preparation method of the nitrocellulose membrane in Example 28 is as follows:

[0199] S1. Prepare the casting solution, which by weight includes 20 parts nitrocellulose, 80 parts organic solvent, 20 parts Tween 60, and 6 parts glycerol; the organic solvent is acetone.

[0200] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 40℃, the humidity is controlled at 60%, and the time is 60s.

[0201] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 30s.

[0202] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0203] The preparation method of the nitrocellulose membrane in Example 29 is as follows:

[0204] S1. Prepare the casting solution, which by weight includes 15 parts nitrocellulose, 80 parts organic solvent, 5 parts Tween 60, and 5 parts glycerol; the organic solvent is acetone.

[0205] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 25°C, the humidity is controlled at 30%, and the time is 120s.

[0206] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 25℃, and the processing time is 180s.

[0207] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0208] The preparation method of the nitrocellulose membrane in Example 30 is as follows:

[0209] S1. Prepare the casting solution, which includes 12 parts by weight of nitrocellulose, 80 parts of organic solvent, 10 parts of Tween 60, and 0.1 parts of glycerol; the organic solvent is acetone.

[0210] S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. In this step, the temperature is 20°C, the humidity is controlled at 40%, and the time is 45s.

[0211] S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. The coagulation bath is a sodium chloride solution with a mass concentration of 0.5%, the temperature is 20℃, and the processing time is 240s.

[0212] S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

[0213] The strips from Examples 1-30 were subjected to streak testing and prepared into test strips for protein immunochromatographic detection. The specific preparation methods are as follows:

[0214] 1. The prepared nitrocellulose membrane was streaked to draw the test line and the control line. The control line used goat anti-mouse IgG polyclonal antibody, and the test line used hepatitis B virus monoclonal antibody 1.

[0215] 2. The nitrocellulose membrane after marking is cut and spread and fixed on the substrate material to obtain the reaction zone. In this application, the substrate material is a polyester board.

[0216] 3. A color developer pad is placed at one end of the reaction zone. In this embodiment, the color developer pad uses a microporous membrane structure. In this application, a polypropylene fiber membrane is selected. The preparation method of the color developer pad is as follows:

[0217] The chromogenic reagent solution was adjusted to pH 10 using potassium carbonate. The labeled antibody was added to the solution, and the reaction was carried out with shaking at room temperature. The surface of the chromogenic reagent was then blocked with BSA, followed by centrifugation and washing to obtain the gold-labeled complex. This gold-labeled complex was then sprayed onto a chromogenic reagent pad. In this embodiment, the selected chromogenic reagent particles were colloidal gold with a particle size range of 40–60 nm, and the labeled antibody was hepatitis B virus monoclonal antibody 2.

[0218] 4. Lay a sample pad on the outside of the color developer pad. The sample pad is a glass fiber membrane.

[0219] 5. Lay an absorbent pad at the other end of the reaction zone.

[0220] It should be noted that the use of hepatitis B surface antigen in this application is merely for illustrative purposes. In practice, different antigens can also be detected by using different antibodies.

[0221] In this embodiment, different protein chromatography test strips obtained in different embodiments are used, and the test strips are tested. The specific detection method is as follows:

[0222] Hepatitis B surface antigen (HBsAg) buffer solution was prepared using a 10M PBS system. 0.05% (w / w) Triton and a suitable amount of surfactant were added to prepare a HBsAg concentration of 100 ng / mL. The prepared HBsAg buffer solution was then dropped onto a sample pad for detection. In addition, norovirus and adenovirus were added as negative control groups. The concentration of each control group was 1000 ng / mL. During the detection process, the background color outside the C-line and T-line was observed and recorded as +++, ++, + (from darkest to lightest), with almost no background color recorded as -.

[0223] The results of the tests conducted on Examples 1 to 30 are shown in Table 2.

[0224] Table 2

[0225]

[0226]

[0227] The experimental data clearly show that the nitrocellulose membranes prepared in this application can be used reasonably well in the field of protein immunochromatographic detection, exhibiting good selectivity and transferability. Overall, the membrane creep rate is around 90 s / 4 cm, and the creep rate is mainly positively correlated with the average pore size of the membrane surface. This nitrocellulose membrane has a relatively small surface SEM pore size, resulting in a low overall creep rate, making it suitable for colloidal gold particles with small average particle sizes.

[0228] In the above embodiments, firstly, in Embodiments 14 and 29, the K1 value is significantly too large. The K1 value is the value of (N1·R13) / D1. When it is too large, it means that compared with the pore size of the fiber surface, the nitrocellulose membrane has an excessive number of nodes and node diameter. That is, the nodes cover an excessively large surface area. The most obvious result is that the surface scribing is uneven, and the background color becomes darker. This is because the excessive node coverage will cause the liquid flow to be obstructed, affecting the material transport, which is also the reason for the darker background color. Based on the above, although K1 in Embodiment 7 is within an acceptable range, the K2 value is relatively large. Within this range, although the number and size of nodes are controlled within a certain range, it is still relatively large compared with R2. Similarly, an excessively large specific surface area will be formed in the system, resulting in a slightly darker background depth.

[0229] In contrast, Examples 8, 10, and 13 have lower K1 values. When K1 is too low, on the one hand, the membrane surface has poor material retention capacity, specifically manifested in the tendency for scribing to turn white. On the other hand, since controlling the number of nodes to a very low level is actually quite difficult, Examples 10 and 13 share a significant characteristic: the diameter of the fiber nodes is very small. This results in an excessively large specific surface area in the node distribution region, thereby increasing the non-specific adsorption of the membrane in local areas. Consequently, although Examples 10 and 13 have a lighter overall background color, color patches still form in local areas. Based on the above, although K1 in Example 20 is within the range, the K2 value is too low, which also produces a similar effect. The whitening phenomenon is not obvious, but a relatively dark background color still exists overall. This demonstrates that even when controlling the number and diameter of nodes within a specific range, it is still necessary to maintain a specific relationship between the node diameter and the fiber diameter; otherwise, adverse effects can easily occur, affecting the accuracy of the detection.

[0230] Furthermore, based on the above, in Example 6, the diameter of the nodes was relatively large. Although the overall porosity was large, the increased node diameter still resulted in a significant whitening effect, and the excessively large node diameter significantly affected the uniformity of the chromatography process. While Examples 22 and 23 had significantly smaller node diameters, the values ​​of P2·D1 / R1 and K3 were also small in both examples. This means that although the number of nodes and the particle size were not large, the main areas where the nodes were present covered the fibers, which easily affected the fiber's flow conductivity. This resulted in non-uniform chromatography and jagged lines in the scribing area. In Example 26, there was a large number of nodes and an excessively large K3 value. The nodes formed an excessively large volume within the system, hindering the flow of the colloidal gold system and introducing greater non-uniformity, with a more pronounced whitening effect in the scribing area.

[0231] In Example 30, a nitrocellulose membrane with a fine fiber diameter and a low R1 / D1 value was prepared by adjusting experimental parameters. Due to the fine fiber diameter, charge imbalance easily occurs within the nitrocellulose membrane when the liquid flows through it, leading to adsorption of some colloidal gold and protein systems, resulting in a slight background color. In Examples 11 and 12, excessively coarse fiber systems were prepared. When the fibers are too coarse, the capillary effect is slightly weakened, which has a certain impact on the overall flow rate. Furthermore, the loading and binding capacity of proteins are somewhat reduced. During scribing, the liquid easily flows away through the gaps in the fibers, thus weakening the binding performance of the material in the scribed area. The resulting phenomena are a whitish and uneven scribing pattern and a reduced flow rate.

[0232] In Examples 9 and 21, both exhibited relatively large R1 / D1 values. In Example 21, a significant area of ​​the fiber surface was covered by nodes. These properties indicate that the nodes, compared to pores and fibers, formed a larger resistance system and blocking structure. Although this did not significantly affect the liquid flow rate, it significantly impeded the protein and colloidal gold systems, resulting in a darker background color. Furthermore, the excessive distribution of nodes in the scribed areas caused a degree of jaggedness. In Examples 2, 11, and 28, even when other parameters met the requirements, an excessive number of nodes were still formed. In this state, the overall uniformity and flowability were good, but it still caused some impediment and non-specific adsorption of proteins and colloidal gold, producing a certain background color under specific conditions.

[0233] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A nitrocellulose membrane, formed by nitrocellulose fibers interwoven into a network structure, and having internal channels for liquid passage, characterized in that, The fiber has nodes on the outer surface, and the number of node distribution per unit area N1, the average diameter of the nodes R1 and the average SEM pore size D1 of the outer surface satisfy the following relationship: N1·R1 3 =D1·K1, wherein K1 is in the range of 3-20%. The average diameter R2 of the fiber is 2-3 μm; the average diameter R1 of the node is 4-7 μm; and the average SEM pore size D1 of the outer surface is 6.42-13.70 μm. The number of nodes per unit area N1 and the average node diameter R1 have the following relationship: N1·R1 2 =K3; where K3 ranges from 0.1 to 0.26 μm, and the number of nodes per unit area N1 is no greater than 15 per (50 μm). 2 .

2. The nitrocellulose membrane according to claim 1, characterized in that, The value of K1 and the average diameter R2 of the fiber satisfy the following relationship: K1 = K2·R2 2 The value of K2 ranges from 0.6 to 3.0%.

3. A nitrocellulose membrane according to claim 2, characterized in that, The ratio of the average node diameter R1 on the outer surface to the average SEM aperture diameter D1 on the outer surface is not greater than 0.

66.

4. A nitrocellulose membrane according to claim 1, characterized in that, On the nitrocellulose fiber, the proportion P2 of the length covered by the knot to the total length of the nitrocellulose fiber is 3 to 6.5%.

5. A nitrocellulose membrane according to claim 4, characterized in that, The proportion P2 of the length covered by the knot to the total length of the nitrocellulose fiber has the following relationship with the ratio P3 between the fiber diameter and the knot diameter: P2∶P3=6~12%.

6. The method for preparing the nitrocellulose membrane according to any one of claims 1 to 5, characterized in that, It includes the following steps: S1. Prepare the casting solution, which includes 5-20 parts by weight of nitrocellulose, 80 parts of organic solvent, 5-20 parts of nonionic surfactant, and 0.1-10 parts of aliphatic polyol. S2. The casting solution is applied to the substrate material and subjected to evaporation and phase separation pretreatment to obtain the first initial film. S3. The first intermediate product is immersed in a coagulation bath for phase separation to obtain the second primary film. S4. The above system is immersed in an aqueous solution for cleaning, and then dried to obtain a nitrocellulose membrane.

7. The method for preparing nitrocellulose membrane according to claim 6, characterized in that, In step S2, the temperature is controlled at 15–30°C, the humidity at 30–50%, and the time at 1–60 seconds.

8. The method for preparing nitrocellulose membrane according to claim 6, characterized in that, In step S3, a sodium chloride solution with a mass concentration of 0.1% to 1% is selected as the coagulation bath.

9. The method for preparing nitrocellulose membrane according to claim 6, characterized in that, In step S3, the temperature is controlled at 10–30°C and the phase separation time is 20–600 s.

10. The nitrocellulose membrane according to claim 6, characterized in that, The aliphatic polyol is glycerol, and the glycerol has a mass fraction of 1 to 5 parts.

11. The use of the nitrocellulose membrane according to any one of claims 1 to 5 in the field of immunochromatography.

Citation Information

Patent Citations