A method for granulating, calcining and decomposing phosphogypsum

Through the phosphogypsum granulation, calcination and decomposition method, granulation technology and additives are used to achieve efficient decomposition of phosphogypsum and collection of sulfuric acid tail gas, solving the environmental threats and resource waste problems in phosphogypsum treatment, reducing energy consumption and improving improve product strength.

CN117865512BActive Publication Date: 2024-10-18YIDU XINGFA CHEMICAL CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311691657.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2024-10-18
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

The treatment and utilization of phosphogypsum poses environmental threats and waste of resources. The SO2 concentration in the preparation of sulfuric acid in the existing technology is low, and the product performance after calcining phosphogypsum is inferior to that of natural gypsum, and the calcining temperature is high energy-consuming and difficult to effectively decompose.

Method used

Using granulation technology, dry phosphogypsum is mixed with reducing agents and auxiliaries, and is preliminarily calcined at low temperature to generate semi-hydrated gypsum, which is then granulated and further calcined at high temperature. Granulation equipment is used to achieve rapid decomposition of phosphogypsum to produce high-quality gypsum. Intensely calcine the balls and collect the sulfuric acid tail gas.

Benefits of technology

It reduces the calcination temperature and time, saves energy consumption, increases the decomposition rate of phosphogypsum, ensures the purity and strength of the material, avoids the generation of dust, and expands the application direction.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a method for granulating, calcining and decomposing phosphogypsum, which comprises the following steps: firstly, calcining and converting the phosphogypsum into semi-hydrated gypsum, adding a reducing agent, mixing a part of the raw gypsum which has not been calcined, and granulating the material by utilizing the adhesiveness of the semi-hydrated gypsum itself through granulation; and finally, placing the gypsum particles into a rotary kiln, calcining the gypsum under the condition of introducing an atmosphere, and quickly reducing the phosphogypsum into calcined balls and sulfur dioxide which are valuable in the field of building materials, thereby decomposing the phosphogypsum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste utilization, in particular to the treatment and utilization of phosphogypsum, and in particular to a method for granulating, calcining and decomposing phosphogypsum. Background Art

[0002] Phosphogypsum is a solid waste residue produced during the production of wet phosphoric acid. Its main component is calcium sulfate dihydrate. 4.5~5 tons of phosphogypsum are produced as a by-product for every ton of phosphoric acid produced. Phosphogypsum has a complex composition and is acidic. It is difficult to manage comprehensively and poses a great threat to the environment. Sulfuric acid is widely used in the chemical industry. 60% of sulfuric acid in my country is used for phosphate fertilizer production. About 1.5 tons of sulfuric acid is consumed for every ton of phosphoric acid produced. At present, the main raw material for sulfuric acid production in my country is sulfur. However, due to the shortage of sulfur resources in my country, sulfuric acid is mainly produced by importing sulfur. Therefore, the rational development and utilization of sulfur resources has become one of the key issues of the chemical industry. Phosphogypsum contains sulfur and calcium elements and can be used to produce sulfuric acid. The decomposition and acid production systems of phosphogypsum mainly include carbon reduction, sulfur reduction, and reducing gas methods.

[0003] CN108002724A discloses a two-step calcination method for preparing phosphogypsum-based cementitious materials, wherein the phosphogypsum is subjected to water washing and acid washing treatment to achieve deep purification of the phosphogypsum, and then fly ash and activated carbon are mixed and ground, and then subjected to two-stage calcination of rapid dehydration and high-temperature sintering under a reducing atmosphere to obtain the phosphogypsum-based cementitious materials. The phosphogypsum is treated with water washing and acid washing to remove harmful impurities that affect the application performance of the cementitious materials. The obtained phosphogypsum has no price advantage over natural gypsum, and the product performance is still different.

[0004] CN112358212A discloses a method for comprehensive utilization of phosphogypsum, wherein bauxite powder is added to phosphogypsum, coal powder is stirred evenly, and then formed into balls and placed in a calcining device, and then the calcining device is sent to a tunnel kiln, and flue gas is collected for sulfuric acid preparation, and the calcined balls are used as ceramsite; the method has the characteristics of being able to efficiently and comprehensively utilize phosphogypsum to produce sulfuric acid and ceramsite. In this scheme, phosphogypsum is directly calcined, and the SO2 concentration in the collected flue gas is low. Summary of the invention

[0005] The present invention provides a method for granulating, calcining and decomposing phosphogypsum. In the form of calcination, a part of dry phosphogypsum is mixed with a reducing agent and a reducing aid, and then with the calcined hemihydrate gypsum, through a granulating device to obtain gypsum balls that are evenly mixed and have a certain strength. Then, through the last step of calcination, the phosphogypsum is quickly decomposed into calcined balls with higher strength, thereby achieving the decomposition of the phosphogypsum.

[0006] The technical solution of the present invention is a method for granulating, calcining and decomposing phosphogypsum, comprising the following steps:

[0007] S1. Placing the phosphogypsum raw material in a calcining furnace and calcining it for a period of time at a calcining temperature of 160°C to 200°C to obtain calcined slag, i.e., hemihydrate gypsum;

[0008] S2, adding a reducing agent and an auxiliary agent to part of the hemihydrate gypsum obtained in S1, and mixing a considerable portion of the raw phosphogypsum that has not been calcined, and after adding a certain proportion of water, granulating the mixture to obtain phosphogypsum balls with a certain strength;

[0009] S3. The phosphogypsum obtained in S2 is put into a rotary kiln and calcined at a high temperature of 950°C to 1100°C under the condition of introducing an atmosphere, so that the phosphogypsum is quickly reduced to sulfur dioxide and calcined balls, thereby achieving the decomposition of the phosphogypsum.

[0010] Furthermore, the water content of the phosphogypsum raw material in S1 is 10-15wt%. The attached water and part of the crystal water of the phosphogypsum are removed after calcination.

[0011] Furthermore, the temperature of the first stage calcination is 160°C to 200°C.

[0012] Furthermore, the calcination time is 20 to 40 minutes.

[0013] Furthermore, the mass ratio of the first-stage calcined slag to the uncalcined raw phosphogypsum in S2 is 1:1~5.

[0014] Furthermore, the amount of water added to S2 is 0.14-0.6 of the weight of the hemihydrate gypsum slag and the uncalcined raw phosphogypsum.

[0015] Furthermore, the reducing agent in S2 is coke powder; the preferred amount is 0.2~0.257 of the total weight of the hemihydrate gypsum slag and the uncalcined raw phosphogypsum in S2.

[0016] Furthermore, the auxiliary agent in S2 is fly ash; the preferred amount is 0.12~0.2 of the total weight of the hemihydrate gypsum slag and the uncalcined raw phosphogypsum in S2.

[0017] Furthermore, the granulation equipment is a disc granulator or an extrusion granulator.

[0018] Furthermore, the calcination time in S3 is 20 to 40 minutes.

[0019] Furthermore, the atmosphere introduced into S3 is nitrogen.

[0020] Furthermore, the calcination time in S3 is 30 to 60 minutes.

[0021] The present invention comprises three steps, wherein the first step is to calcine at a temperature of 160°C to 200°C, and its main purpose is to remove part of the crystal water in the phosphogypsum; the second step is to add a certain amount of reducing agent and auxiliary agent, and obtain gypsum balls with a certain strength under the action of granulating equipment; the addition of auxiliary agent helps to shorten the temperature and time of calcining and decomposing the phosphogypsum, and the phosphogypsum can be decomposed to generate CaO and SO2 at 950°C to 1100°C, and CaSO4 is converted into CaO under the action of C, and the generation of CaS can be reduced in a nitrogen atmosphere; after calcining, calcined balls with higher strength and tail gas for preparing sulfuric acid are finally obtained, and in a moving state, granulation and calcination have the advantages of rapid collection, concentrated reaction and avoidance of dust and the like.

[0022] The main reactions of the calcination process are as follows:

[0023] CaSO4+2C=CaS+2CO2

[0024] CaS+3CaSO4=4CaO+4SO2

[0025] 2CaSO4+3C=2CaO+2S+3CO2

[0026] 2CaSO4=2CaO+O2+2SO2

[0027] CaSO4+CO=CaO+CO2+SO2

[0028] The beneficial effects of the present invention are:

[0029] (1) The calcination temperature of the present invention is generally low and the time is short. The first step of calcination is to produce hemihydrate gypsum. At this time, the temperature is low and the energy consumption is small. The calcination time is short, especially the calcination time of the decomposition step, which saves energy.

[0030] (2) The present invention promotes the reduction of decomposition temperature during the calcination and decomposition process by adding auxiliary agents, thereby shortening the calcination temperature and improving the decomposition rate of phosphogypsum.

[0031] (3) The present invention uses a granulation device to prepare gypsum into particles by utilizing the adhesiveness of hemihydrate gypsum itself, thereby ensuring the purity of the material and avoiding the occurrence of stratification or uneven contact of the material during the moving calcination state.

[0032] (4) The present invention utilizes fly ash as a reducing agent, which not only plays a role in decomposing gypsum, but also increases the strength of the final calcined balls, thereby expanding the final application direction. DETAILED DESCRIPTION

[0033] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0034] The main components of the phosphogypsum raw materials used in the following cases are calcium sulfate dihydrate (92.4%) and silicon dioxide (5.3%).

[0035] Example 1

[0036] The phosphogypsum is crushed, ground and passed through a 100-mesh sieve.

[0037] 1) Calcine the phosphogypsum at 180℃±10℃ for 30min to obtain semi-hydrated gypsum slag; place the fly ash and coke powder in an oven at 40~50℃ to dry;

[0038] 2) Mix semi-hydrated gypsum slag and original gypsum in a mass ratio of 1:3, mix dry coke powder and mixed gypsum in a mass ratio of 0.2:1, and then add fly ash and mix well. The mass ratio of fly ash to mixed gypsum is 0.12:1. The fly ash is wrapped in gypsum particles to obtain uniform spheres.

[0039] 3) The obtained granular material is placed in a rotary kiln with a nitrogen atmosphere, and the temperature is raised to 1000℃ for calcination under rotating conditions, and the temperature is kept for 40 minutes. After the calcination is completed, the material is taken out and remains in its original shape, and naturally cooled to room temperature, and the SO4 content in the residue is determined. 2- The content is 0.64%, and the amount of calcium sulfate in the residue is calculated to be 0.91%.

[0040] The decomposition rate of calcium sulfate can be calculated according to the following formula:

[0041] Phosphogypsum decomposition rate φ = (1-residual CaSO4 / total amount of CaSO4 in the sample) × 100%

[0042] The decomposition rate of phosphogypsum in this embodiment was determined to be 99.53%.

[0043] Example 2

[0044] The phosphogypsum is crushed, ground, and passed through a 100-mesh sieve. 1) Dry coke powder and phosphogypsum are mixed evenly at a mass ratio of 0.2:1, and then fly ash is added and mixed evenly. The mass ratio of fly ash to phosphogypsum is 0.12:1. After adding 40% water, granulation is performed to make the gypsum into balls to obtain uniform balls;

[0045] 2) The uniform spheres were placed in a rotary kiln with a nitrogen atmosphere, heated to 1000°C for calcination under rotating conditions, and kept at this temperature for 40 minutes. After the calcination, the material was taken out and kept in its original shape, and naturally cooled to room temperature. The SO4 content in the residue was determined.2- The content is 10.42%, and the content of calcium sulfate in the residue is calculated to be 14.89%. The material is broken into small pieces and powder during the transfer process.

[0046] The decomposition rate of phosphogypsum in this embodiment was determined to be 91.79%.

[0047] By comparing Example 1 with Example 2, it can be seen that when granulation is performed without calcination to hemihydrate gypsum, the material does not have strength after the experiment. This is because the presence of hemihydrate gypsum provides early strength.

[0048] Example 3

[0049] Based on Example 1, the difference is that the mass ratio of fly ash to mixed gypsum is 0.12:1, the fly ash is wrapped by gypsum outside the particles, and after obtaining uniform spheres, a calcination experiment is carried out at 1000°C for 40 minutes, and the result is 9.53% sulfate.

[0050] The amount of calcium sulfate in the residue was 13.6%.

[0051] The decomposition rate of phosphogypsum in this embodiment is 90.75% as determined by calculation.

[0052] By comparing Example 3 with Example 1, it can be seen that the experimental result of wrapping the fly ash in the outer layer has a lower reaction result than wrapping it in the inner layer. This is because the inner layer is denser and the reaction is not thorough enough.

[0053] Example 4

[0054] Based on Example 1, the difference is that: the semi-hydrated gypsum slag and the original gypsum are mixed in a mass ratio of 1:3, the dry coke powder and the mixed gypsum are mixed in a mass ratio of 0.2:1, granulated, and a uniform sphere is obtained. After the calcination experiment is carried out under the conditions of 1000°C and 40min, the results are as follows: the sulfate content is 22.54%, and the calcium sulfate content is 32.17%

[0055] The decomposition rate of phosphogypsum in this embodiment was determined to be 78.14%.

[0056] By comparing Example 4 with Example 1, it can be seen that the experimental results without adding fly ash are lower. This is because the silicon dioxide and metal oxides contained in the fly ash have a positive effect on the decomposition of gypsum.

[0057] Example 5

[0058] Based on Example 1, the differences are: 2) Hemihydrate gypsum slag and raw gypsum are mixed evenly in a mass ratio of 1:3, dry coke powder and mixed gypsum are mixed evenly in a mass ratio of 0.2:1, and then fly ash is added and mixed evenly, the mass ratio of fly ash to mixed gypsum is 0.12:1, and a calcination experiment is carried out at 1000°C for 40min.

[0059] The content of sulfate in the residue is 45.8%, calcium sulfate is 65.45%, and the decomposition rate of phosphogypsum is 50.58%

[0060] By comparing Example 5 with Example 1, it can be seen that when gypsum and reducing agent and reducing aid are closely mixed without granulation, stratification of materials may occur during the movement process, which affects the decomposition effect.

[0061] Example 6

[0062] Compared with Example 1, in step 2, the semi-hydrated gypsum slag and the original gypsum are mixed evenly in a mass ratio of 1:4, the dry fly ash and the mixed gypsum are mixed evenly in a mass ratio of 0.15:1, and the final calcination temperature is 950° C., and the rest is the same as Example 1, and the calculated decomposition rate is 77.63%.

[0063] By comparing Example 6 with Example 1, it can be seen that lowering the calcination temperature is not conducive to the decomposition reaction.

[0064] Example 7

[0065] Based on Example 1, the difference is that: step 3) the calcination time is reduced to 30 minutes, and the rest is the same as Example 2, and the calculated decomposition rate is 64.3%.

[0066] By comparing Example 7 with Example 1, it can be seen that reducing the calcination time will lead to insufficient reaction.

[0067] Example 9

[0068] Based on Example 1, the difference is that: step 3) the calcination temperature is 1100° C., and the rest is the same as Example 1, and the calculated decomposition rate is 99.69%.

[0069] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. A method for granulating, calcining and decomposing phosphogypsum, characterized in that: The following steps are involved: S1. Placing the phosphogypsum raw material in a calcining furnace for a period of calcination, wherein the calcination time is 20 to 40 minutes and the calcination temperature is 160°C to 200°C to obtain calcined slag, i.e., hemihydrate gypsum; S2. Add reducing agent coke powder to part of the calcined slag obtained in S1, and mix with uncalcined phosphogypsum raw material, mix evenly to obtain mixed gypsum, and then add auxiliary fly ash, and obtain phosphogypsum balls by granulation. The amount of coke powder is 0.2~0.257 of the total weight of the semi-hydrated gypsum slag and the original phosphogypsum, and the amount of auxiliary agent is 0.12~0.2 of the total weight of the semi-hydrated gypsum slag and the original phosphogypsum. The fly ash is wrapped in gypsum particles to obtain uniform spheres. The mass ratio of the semi-hydrated gypsum slag to the uncalcined original phosphogypsum is 1:1~5. S3. Put the phosphogypsum balls obtained in S2 into a rotary kiln, and carry out two-stage calcination under the condition of passing an atmosphere. The atmosphere is nitrogen and the calcination temperature is 950℃~1100℃ to achieve the decomposition of the phosphogypsum.

2. The method according to claim 1, characterized in that: In step S1, the water content in the phosphogypsum raw material is 10-15wt%.

3. The method according to claim 1, characterized in that: In step S2, the granulation equipment is a disc granulator or an extrusion granulator.

4. The method according to claim 1, characterized in that: The second stage calcination temperature in S3 is 950°C to 1100°C, and the calcination time is 30 to 60 minutes.

Citation Information

Patent Citations

  • Method for preparing phosphogypsum base cementing material by two-step calcining

    CN108002724A

  • Comprehensive utilization method of phosphogypsum

    CN112358212A

  • Production process for preparing calcium oxide and sulfur dioxide by decomposing ardealite

    CN101602518A

  • Process of sulfuic acid from supse

    CN1040009A