Antibacterial gypsum board and its preparation method
By combining a loaded composite antibacterial agent and a Cu2O/ZnO antibacterial agent, the problem of easy leakage of plant-derived antibacterial agents was solved, and antibacterial gypsum board with excellent and stable antibacterial effect was prepared, improving the antibacterial and mechanical properties of gypsum board.
Patent Information
- Application Number
- CN202410029766.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-09
AI Technical Summary
Existing plant-derived antibacterial agents are liquids, which are prone to leakage and cause the antibacterial components to be lost too quickly, resulting in unstable antibacterial effects.
A supported composite antibacterial agent is used, and the composite antibacterial dispersion is loaded onto a modified porous material, combined with Cu2O/ZnO antibacterial agent to enhance the antibacterial effect and improve stability.
The prepared antibacterial gypsum board has excellent antibacterial effects against Staphylococcus aureus and Escherichia coli, with excellent and stable antibacterial properties, good mechanical properties, and extended antibacterial life.
Smart Images

Figure BDA0004655698110000061 
Figure BDA0004655698110000071
Abstract
Description
Technical Field
[0001] This application relates to the field of building materials technology, and in particular to an antibacterial gypsum board and its preparation method. Background Technology
[0002] Plant-based antibacterial agents are bio-based materials, all-natural and environmentally friendly, with excellent antibacterial effects; they also have a unique fragrance that can soothe emotions. To enhance the antibacterial effect of plant-based antibacterial agents, they are compounded with inorganic metal oxides. However, the compound antibacterial agent is a liquid, which has drawbacks such as easy leakage and rapid loss of antibacterial components.
[0003] Therefore, there is a need for an antibacterial gypsum board with enhanced and durable antibacterial effects and a method for manufacturing it. Summary of the Invention
[0004] The following is an overview of the subject matter described in detail in this application. This overview is not intended to limit the scope of the claims.
[0005] In one aspect, this application provides an antibacterial gypsum board, comprising, by weight, 1000 parts of gypsum clinker, 5-50 parts of a loaded composite antibacterial agent, 4-8 parts of starch, and 600-800 parts of water. The loaded composite antibacterial agent comprises, by weight, 5-10 parts of a composite antibacterial dispersion and 5-10 parts of a modified porous material. The composite antibacterial dispersion comprises, by weight, 4-6 parts of a plant-derived antibacterial agent, 0.5-1.5 parts of anionic modifier, 0.5-2 parts of Cu2O / ZnO antibacterial agent, and 0.1-0.5 parts of emulsifier.
[0006] In some embodiments, the modified porous material comprises, by weight, 10-15 parts of porous material, 0.5-2 parts of cationic modifier, 50-100 parts of anhydrous ethanol and 40-100 parts of water.
[0007] In some embodiments, the Cu2O / ZnO antibacterial agent comprises, by weight, 0.5-2 parts of ZnO, 1-2 parts of disodium ethylenediaminetetraacetate, 1-2 parts of copper sulfate pentahydrate, and 1-3 parts of 0.1 mol / L ascorbic acid solution.
[0008] In some embodiments, the porous material is selected from the group consisting of diatomaceous earth, montmorillonite, kaolinite, halloysite, expanded perlite, and expanded graphite.
[0009] In some embodiments, the cationic modifier is selected from the group consisting of hexadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, dodecyldimethylamine oxide, and cationic silicone oil.
[0010] In some embodiments, the plant-derived antibacterial agent is selected from the group consisting of Artemisia argyi essential oil, peppermint essential oil, eucalyptus essential oil, lavender essential oil, rose essential oil, cypress essential oil, and cinnamon essential oil; the emulsifier is Tween 80 or Span 80; the gypsum clinker is selected from the group consisting of desulfurized gypsum, phosphogypsum, and natural gypsum; and the water is distilled water or deionized water.
[0011] In some embodiments, the anionic modifier is selected from the group consisting of dodecyl sulfate, sodium dodecylbenzenesulfonate, sodium stearate, and sodium lauroyl sarcosinate.
[0012] On the other hand, this application also provides a method for preparing antibacterial gypsum board, comprising the following steps:
[0013] Add 1000 parts by weight of gypsum clinker, 4-8 parts by weight of starch, and 5-50 parts by weight of loaded composite antibacterial agent to 600-800 parts by weight of water, and mix evenly until the slurry begins to thicken; after the slurry is shaped, dried, and trimmed, the antibacterial gypsum board is obtained.
[0014] The supported composite antibacterial agent is prepared through the following steps:
[0015] At room temperature, 5-10 parts by weight of the composite antibacterial dispersion are added to 5-10 parts by weight of the modified porous material while grinding. The mixture is then allowed to stand under vacuum. This process is repeated 2-3 times to obtain a mixture.
[0016] The mixture is refrigerated and centrifuged to remove excess essential oil from the surface, thus obtaining a loaded composite antibacterial agent;
[0017] The composite antibacterial dispersion is prepared by the following steps:
[0018] Mix and stir 4-6 parts by weight of plant-derived antibacterial agent and 0.5-1.5 parts by weight of anionic modifier until fully dispersed to obtain the first mixed solution;
[0019] Add 0.5-2 parts by weight of Cu2O / ZnO antibacterial agent to the first mixed solution, sonicate and mix to obtain a dispersion; and
[0020] Add 0.1-0.5 parts by weight of emulsifier to the dispersion, stir and emulsify to obtain the composite antibacterial dispersion.
[0021] In some embodiments, the Cu2O / ZnO antibacterial agent is prepared by the following steps:
[0022] Add 0.5-2 parts by weight of ZnO to 30-50 parts of water, stir and sonicate to obtain a suspension;
[0023] Add 1-2 parts by weight of disodium ethylenediaminetetraacetate to the suspension and stir;
[0024] Add 1-2 parts by weight of copper sulfate pentahydrate, condense and reflux to obtain a second mixed solution;
[0025] Add 1-3 parts by weight of 0.1 mol / L ascorbic acid solution to the second mixed solution to reduce copper ions to Cu. + The third mixed solution was obtained;
[0026] The third mixed solution is separated by centrifugation and rinsed with deionized water to obtain the Cu2O / ZnO antibacterial agent.
[0027] In some embodiments, the modified porous material is prepared by the following steps:
[0028] Mix 10-15 parts by weight of porous material with 50-100 parts by weight of ethanol aqueous solution and stir to fully swell it to obtain a suspension. The weight ratio of anhydrous ethanol to water in the ethanol aqueous solution is in the range of 1:1 to 1:2.
[0029] Mix and stir 0.5-2 parts by weight of the cationic modifier with 50-60 parts by weight of water to obtain a cationic modifier solution;
[0030] The modifier solution was added dropwise to the suspension, stirred and centrifuged, and the resulting solid material was diluted with deionized water, centrifuged and washed to obtain the solid material.
[0031] Dry the solid material;
[0032] The modified porous material is obtained by crushing and sieving the dried solid material.
[0033] This application enhances the dispersibility of antibacterial agents by combining plant-derived antibacterial agents with Cu2O / ZnO antibacterial agents, resulting in gypsum boards with excellent antibacterial effects. Specifically, the antibacterial gypsum board of this application exhibits good antibacterial effects against Staphylococcus aureus and Escherichia coli.
[0034] This application effectively improves the storage stability of antibacterial materials by loading a composite antibacterial dispersion with a modified porous material, reduces the contact between plant-derived antibacterial agents and gypsum, and achieves the goal of simultaneously improving the antibacterial and mechanical properties of gypsum board.
[0035] Other features and advantages of this application will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the application. Other advantages of this application may be realized and obtained by means of the methods described in the description. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of this application clearer, the embodiments of this application are described in detail below. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be arbitrarily combined with each other.
[0037] Unless otherwise specified, all materials used in the following examples and comparative examples are commercially available materials.
[0038] Example 1
[0039] (1) Add 1g of ZnO to 40ml of deionized water, stir magnetically for 30min at 20℃, and then sonicate for 10min to obtain a suspension;
[0040] (2) Slowly add 1.2g of disodium ethylenediaminetetraacetate to the suspension obtained in step (1) and stir at a constant temperature of 40°C for 3 hours;
[0041] (3) Add 1.5g of copper sulfate pentahydrate to the solution obtained in step (2) and reflux at 45°C for 30min.
[0042] (4) Add 1.76g of ascorbic acid to 100ml of deionized water and disperse evenly to prepare a 0.1mol / L ascorbic acid solution; take 1.8g of the ascorbic acid solution and add it to the solution obtained in step (3) to reduce and chelate copper ions in situ, and continue to stir at a constant temperature for 30min to completely reduce it to Cu. + ;
[0043] (5) The solution obtained in step (4) of centrifugation is rinsed with deionized water to obtain Cu2O / ZnO antibacterial agent;
[0044] (6) Take 5g of essential oil and put it into a magnetic stirrer. Add 0.5g of anionic modifier sodium dodecyl sulfate (SDS) and stir at room temperature for 30 minutes to disperse it fully.
[0045] (7) Take 1g of Cu2O / ZnO antibacterial agent and add it to the solution obtained in step (6). Sonicate for 10min, keep the temperature at 30℃ and stir for 30min to fully mix and obtain a dispersion.
[0046] (8) Take 0.3g of Tween 80 and add it to the dispersion prepared in step (7). Stir for 3 hours to fully emulsify and obtain a composite antibacterial dispersion.
[0047] (9) Take 10g of diatomaceous earth into a beaker, add 50g of ethanol aqueous solution (the weight ratio of ethanol to water is 1:1), stir at room temperature for 30min to obtain a suspension.
[0048] (10) Take 1.28g of cationic modifier cetyltrimethylammonium chloride (CTAC), add it to 50ml of deionized water, and stir at 50℃ for 30min to obtain cationic modifier solution;
[0049] (11) Add the cationic modifier solution dropwise to the suspension prepared in step (9), stir at 50°C for 3-6 hours, put the suspension into a centrifuge tube, centrifuge at 4000-4500r / 10min for 10 minutes, dilute the obtained solid material with deionized water, repeat step (11), centrifuge and wash 3-5 times.
[0050] (12) Take out the solid material obtained in step (11) and dry it in an oven at 105°C for 48 hours; crush the dried sample and pass it through a 200-mesh sieve to obtain modified diatomaceous earth;
[0051] (13) Add 5g of the composite antibacterial dispersion obtained in step (8) to 5g of the modified diatomaceous earth obtained in step (12) while grinding at room temperature, place it under vacuum and let it stand for 3 hours. Repeat step (13) 2-3 times to obtain a mixture.
[0052] (14) Transfer the mixture to a 4°C refrigerator and refrigerate for 24 hours. Centrifuge the mixture for 10 minutes to remove excess essential oil from the surface and obtain a loaded composite antibacterial agent.
[0053] (15) Take 10g of the loaded composite antibacterial agent obtained in step (14), 1000g of gypsum clinker, and 5g of starch, mix them evenly, add them to 680g of deionized water, stir in the same direction for 40s until they are evenly mixed, until the slurry begins to thicken.
[0054] (16) Pour the slurry into a flat forming machine with a protective paper, shake to remove air bubbles, press a layer of protective paper on the surface, and form, dry and saw the edges at 40℃±4℃ to obtain antibacterial gypsum board.
[0055] Comparative Example 1
[0056] (1) Take 10g of plant-derived antibacterial agent, 1000g of gypsum powder and 5g of starch, mix them evenly, add them to 680g of deionized water, stir in the same direction for 40s until they are evenly mixed, until the slurry begins to thicken.
[0057] (2) Pour the slurry into a flat forming machine with a protective paper, shake to remove air bubbles, press a layer of protective paper on the surface, form at 40℃±4℃, and obtain antibacterial gypsum board after drying and trimming.
[0058] Comparative Example 2
[0059] (1) Add 1g ZnO to 40ml of deionized water, stir magnetically for 30min at 20℃, and then sonicate for 10min to obtain a suspension;
[0060] (2) Slowly add 1.2g of disodium ethylenediaminetetraacetate to the suspension obtained in step (1) and stir at a constant temperature of 40°C for 3 hours;
[0061] (3) Add 1.5g of copper sulfate pentahydrate to the solution obtained in step (2) and reflux at 45°C for 30 minutes;
[0062] (4) Add 1.76g of ascorbic acid to 100ml of deionized water and disperse evenly to prepare a 0.1mol / L ascorbic acid solution; take 1.8g of the ascorbic acid solution and add it to the solution obtained in step (3) to reduce and chelate copper ions in situ, and continue to stir at a constant temperature for 30min to completely reduce it to Cu. + ;
[0063] (5) The solution obtained in step (4) of centrifugation is rinsed with deionized water to obtain Cu2O / ZnO antibacterial agent;
[0064] (6) Take 5g of essential oil and put it into a magnetic stirrer. Add 0.5g of anionic modifier sodium dodecyl sulfate (SDS) and stir at room temperature for 30 minutes to disperse it fully.
[0065] (7) Take 1g of Cu2O / ZnO antibacterial agent and add it to the solution obtained in step (6). Sonicate for 10min, keep the temperature at 30℃ and stir for 30min to fully mix and obtain a dispersion.
[0066] (8) Take 0.3g of Tween 80 and add it to the dispersion prepared in step (7). Stir for 3 hours to fully emulsify and obtain a composite antibacterial dispersion.
[0067] (9) Take 10g of the composite antibacterial dispersion obtained in step (8), 1000g of gypsum powder, and 5g of starch, mix them evenly, add them to 680g of deionized water, stir in the same direction for 40s until they are evenly mixed, until the slurry begins to thicken.
[0068] (10) Pour the slurry into a flat forming machine with a protective paper, shake to remove air bubbles, press a layer of protective paper on the surface, form at 40℃±4℃, dry and saw the edges to obtain antibacterial gypsum board.
[0069] Performance testing
[0070] The antibacterial properties of the gypsum boards prepared in the examples and comparative examples were tested according to GB T21866-2008, and the test bacteria were Escherichia coli and Staphylococcus aureus. The mechanical properties of the gypsum boards prepared in the examples and comparative examples were tested according to GB 9775-2008, and the test results are shown in Table 1.
[0071] Table 1
[0072]
[0073] Paper bonding performance: Excellent—the entire paper core is firmly bonded; Good—most of the paper core is firmly bonded.
[0074] As shown in Table 1, the loaded composite antibacterial gypsum board prepared in Example 1 exhibits excellent antibacterial properties and good mechanical properties. In Comparative Example 1, the addition of a plant-derived antibacterial agent resulted in some antibacterial properties in the gypsum board, but the addition affected the mechanical properties and the adhesion properties of the facing paper. In Comparative Example 2, a composite antibacterial gypsum board was prepared, and the dispersibility of inorganic materials was improved through interface modification, thus enhancing the antibacterial properties of the gypsum board. However, since the plant-derived antibacterial agent remained in the gypsum interface, the improvement in mechanical properties was not significant. In contrast, Example 1 of this application uses a modified porous material to coat the composite antibacterial agent, effectively improving the storage stability of the antibacterial material and reducing the contact between the plant-derived antibacterial agent and the gypsum, thereby simultaneously improving both the antibacterial and mechanical properties of the gypsum board.
[0075] Furthermore, the antibacterial test results showed that due to the long drying process, the plant-derived antibacterial agent in Comparative Example 1 was severely lost, resulting in poor antibacterial performance and a significant gap between its antibacterial durability and the standard requirements. In Comparative Example 2, the addition of an inorganic antibacterial agent significantly improved the antibacterial performance of the composite antibacterial agent due to its good thermal stability, and it also exhibited excellent durability. In Example 1, the use of porous materials to adsorb the plant-derived material effectively slowed down the volatilization of the plant-derived antibacterial agent, demonstrating a significant synergistic antibacterial effect between the inorganic and plant-derived antibacterial agents, and resulting in higher antibacterial durability.
[0076] Furthermore, regarding the service life of the antibacterial agent material, the gypsum boards prepared in the examples and comparative examples were tested. The gypsum boards prepared in the examples and comparative examples were placed at temperatures of 18-25°C, relative humidity of 40%-70%, and airflow of 400-500 m³ / h. 3 Under the condition of / h, its antibacterial properties were tested after standing for 168h, 336h and 672h, so as to analyze its antibacterial lifespan. The results are shown in Table 2.
[0077] Table 2
[0078]
[0079] As shown in Table 2, the antibacterial properties of all samples decreased. After 672 hours, Comparative Example 1 showed the greatest reduction in antibacterial performance. This is because the antibacterial agent content in the material was low after the plant-derived antibacterial agent volatilized, thus significantly affecting the material's antibacterial performance. Comparative Example 2 showed a relatively large reduction in antibacterial performance, but it performed better than Comparative Example 1. This is because the combination of inorganic antibacterial agents improved the antibacterial stability of the antibacterial material. Example 1 showed the best antibacterial agent stability and the longest antibacterial lifespan. This is because the loading of the porous material slowed down the volatilization of the plant-derived antibacterial agent, improved the synergistic antibacterial effect of the inorganic-plant-derived antibacterial agents, and extended the service life.
[0080] Meanwhile, the inventors of this application also noted that inorganic porous materials have good hydrophilicity but poor lipophilicity, while plant essential oil extracts are mostly large organic molecules that are difficult to dissolve in water, resulting in poor interfacial compatibility with inorganic porous materials and thus easy loss of essential oils. This application improves the interfacial compatibility between the porous material and essential oils by organically modifying the inorganic porous material and introducing organic groups onto the surface of the inorganic clay material. This increases the loading capacity of the porous material for essential oils and enhances the adsorption stability of the porous material for essential oils, thereby significantly extending the service life of the composite antibacterial agent.
[0081] While the embodiments disclosed in this application are as described above, the content is merely for the purpose of facilitating understanding of this application and is not intended to limit this application. Any person skilled in the art to which this application pertains may make any modifications and changes in the form and details of the implementation without departing from the spirit and scope disclosed in this application; however, the scope of protection of this application shall still be determined by the scope defined in the appended claims.
Claims
1. An antibacterial gypsum board, characterized in that, The antibacterial gypsum board, by weight, is prepared from the following materials: 1000 parts of gypsum clinker, 5-50 parts of a loaded composite antibacterial agent, 4-8 parts of starch, and 600-800 parts of water. The loaded composite antibacterial agent, by weight, consists of 5-10 parts of a composite antibacterial dispersion and 5-10 parts of modified porous material. The composite antibacterial dispersion, by weight, consists of 4-6 parts of a plant-derived antibacterial agent, 0.5-1.5 parts of anionic modifier, 0.5-2 parts of Cu2O / ZnO antibacterial agent, and 0.1-0.5 parts of emulsifier. The modified porous material is composed of 10-15 parts of porous material, 0.5-2 parts of cationic modifier, 50-100 parts of anhydrous ethanol and 40-100 parts of water; The Cu2O / ZnO antibacterial agent is composed of 0.5-2 parts ZnO, 1-2 parts disodium ethylenediaminetetraacetate, 1-2 parts copper sulfate pentahydrate, and 1-3 parts 0.1 mol / L ascorbic acid solution. The emulsifier is Tween 80 or Span 80; The Cu2O / ZnO antibacterial agent is prepared by the following steps: Add 0.5-2 parts by weight of ZnO to 30-50 parts of water, stir and sonicate to obtain a suspension; Add 1-2 parts by weight of disodium ethylenediaminetetraacetate to the suspension and stir; Add 1-2 parts by weight of copper sulfate pentahydrate, condense and reflux to obtain a second mixed solution; Add 1-3 parts by weight of 0.1 mol / L ascorbic acid solution to the second mixed solution to reduce copper ions to Cu. + The third mixed solution was obtained; The third mixed solution was separated by centrifugation and rinsed with deionized water to obtain the Cu2O / ZnO antibacterial agent. The plant-derived antibacterial agent is selected from the group consisting of Artemisia argyi essential oil, peppermint essential oil, eucalyptus essential oil, lavender essential oil, rose essential oil, cypress essential oil, and cinnamon essential oil.
2. The antibacterial gypsum board according to claim 1, characterized in that, The porous material is selected from the group consisting of diatomaceous earth, montmorillonite, kaolin, halloysite, expanded perlite, and expanded graphite.
3. The antibacterial gypsum board according to claim 1, characterized in that, The cationic modifier is selected from the group consisting of hexadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, dodecyldimethylamine oxide, and cationic silicone oil.
4. The antibacterial gypsum board according to any one of claims 1-3, characterized in that, The gypsum clinker is selected from the group consisting of desulfurized gypsum, phosphogypsum and natural gypsum; the water is distilled water or deionized water.
5. The antibacterial gypsum board according to any one of claims 1-3, characterized in that, The anionic modifier is selected from the group consisting of dodecyl sulfate, sodium dodecylbenzenesulfonate, sodium stearate, and sodium lauroyl sarcosinate.
6. A method for preparing antibacterial gypsum board according to any one of claims 1-5, characterized in that, Includes the following steps: Add 1000 parts by weight of gypsum clinker, 4-8 parts by weight of starch, and 5-50 parts by weight of loaded composite antibacterial agent to 600-800 parts by weight of water, mix evenly until the slurry begins to thicken; after the slurry is shaped, dried, and trimmed, the antibacterial gypsum board is obtained. The supported composite antibacterial agent is prepared through the following steps: At room temperature, 5-10 parts by weight of the composite antibacterial dispersion are added to 5-10 parts by weight of the modified porous material while grinding. The mixture is then allowed to stand under vacuum. This process is repeated 2-3 times to obtain a mixture. The mixture is refrigerated and centrifuged to remove excess essential oil from the surface, thus obtaining a loaded composite antibacterial agent; The composite antibacterial dispersion is prepared by the following steps: Mix and stir 4-6 parts by weight of plant-derived antibacterial agent and 0.5-1.5 parts by weight of anionic modifier until fully dispersed to obtain the first mixed solution; Add 0.5-2 parts by weight of Cu2O / ZnO antibacterial agent to the first mixed solution, sonicate and mix to obtain a dispersion; and Add 0.1-0.5 parts by weight of emulsifier to the dispersion, stir and emulsify to obtain the composite antibacterial dispersion; The Cu2O / ZnO antibacterial agent is prepared by the following steps: Add 0.5-2 parts by weight of ZnO to 30-50 parts of water, stir and sonicate to obtain a suspension; Add 1-2 parts by weight of disodium ethylenediaminetetraacetate to the suspension and stir; Add 1-2 parts by weight of copper sulfate pentahydrate, condense and reflux to obtain a second mixed solution; Add 1-3 parts by weight of 0.1 mol / L ascorbic acid solution to the second mixed solution to reduce copper ions to Cu. + The third mixed solution was obtained; The third mixed solution was separated by centrifugation and rinsed with deionized water to obtain the Cu2O / ZnO antibacterial agent. The modified porous material is prepared by the following steps: Mix 10-15 parts by weight of porous material with 50-100 parts by weight of ethanol aqueous solution and stir to fully swell it to obtain a suspension. The weight ratio of anhydrous ethanol to water in the ethanol aqueous solution is in the range of 1:1 to 1:
2. Mix and stir 0.5-2 parts by weight of the cationic modifier with 50-60 parts by weight of water to obtain a cationic modifier solution; The modifier solution was added dropwise to the suspension, stirred and centrifuged, and the resulting solid material was diluted with deionized water, centrifuged and washed to obtain the solid material. Dry the solid material; The modified porous material is obtained by crushing and sieving the dried solid material.
Citation Information
Patent Citations
Paper-surfaced gypsum board capable of resisting bacteria and mildew and purifying formaldehyde, and preparation method therefor
WO2021051331A1