A process for making a coating on a product surface

By using a process of combining metal shielding fixtures and heat-resistant tape in narrow areas, the problem of precisely controlling the melting range and tape removal difficulties in the prior art is solved, and the flatness and stability of the spraying area are achieved.

CN117867439BActive Publication Date: 2024-11-08SUZHOU DREAMCHASING ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410108384.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2024-11-08
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

In the field of semiconductor and liquid crystal panels, existing spraying processes are difficult to accurately control the melting range in narrow areas, and conventional masking tapes are difficult to remove and lead to uneven coating edges.

Method used

The metal shielding fixture is used to combine with heat-resistant tape to accurately control the melting range by shielding in non-sprayed areas, and the spraying area is processed using plasma melting technology and machine processing to ensure neat edges.

Benefits of technology

Accurate control of the melting range in narrow areas is achieved, avoiding the problem of difficult tape removal and burrs on the edge of the coating, and ensuring the flatness and stability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117867439B_ABST
    Figure CN117867439B_ABST
Patent Text Reader

Abstract

The present invention discloses a process for making a coating on the surface of a product, wherein the product includes a first area and a convex portion, wherein the convex portion is higher than the first area along a first direction, and the first area includes a spraying area and a shielding area, including: installing a metal shielding fixture to the convex portion of a product component; shielding the side, surface, and product component of the metal shielding fixture with tape that does not require spraying; sandblasting the spraying area; removing the tape shielding the side of the metal shielding fixture; using plasma spraying technology to make a spraying area in the spraying area until the required spraying area thickness; using machining to process the spraying area to the required thickness and shape; and grinding the area on the product component that adheres to the ceramic powder and the area with sharp corners and burrs. The range of spraying can be accurately controlled in a narrow area, avoiding the problem of difficulty in removing the tape after spraying in conventional masking and spraying processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a process for melt spraying on the surface of a product component, and in particular to a process for making a coating on the surface of a product. Background Art

[0002] In the field of semiconductors and liquid crystal panels, since most processes take place in a plasma environment, it is necessary to cover the surface of product components in the machine with a spraying area to provide insulation and protection. Existing spraying areas are usually sprayed onto the product surface through a plasma spraying process.

[0003] In some product parts, there are very narrow steps and other structures that need to be sprayed. The width of these areas is about 2mm or even smaller, and the sprayed areas cannot be connected to the side of the convex part. When using the above conventional process to make the coating, there are the following problems:

[0004] 1. During sandblasting and thermal spraying, the gap between the step and the coating needs to be masked with tape to prevent the coating from sticking to the side of the convex part after thermal spraying. However, since the step height is relatively small and the range to be masked is also very small, the masking range cannot be controlled well during manual masking, and the thermal spraying range cannot be accurately controlled, resulting in the actual thermal spraying range being too large or too small;

[0005] 2. When heat-resistant tape is used to mask the side of the convex part to prevent the coating from sticking to the step, the spraying area formed by the spraying will bury the masking tape, and the masking tape cannot be removed after the spraying area is completed;

[0006] 3. Even if the above problems can be effectively solved, when masking tape is used for masking, the coating material will always be deposited on the tape during spraying. After the tape is removed, the edge where the spraying area contacts the tape will have a zigzag structure, and the coating edge will be uneven. Summary of the invention

[0007] In order to overcome the above disadvantages, the object of the present invention is to provide a process for making a coating on the surface of a product.

[0008] In order to achieve the above purpose, the technical solution adopted by the present invention is: a process for making a coating on the surface of a product, the product includes a first area and a convex portion, the convex portion is higher than the first area along a first direction, the first area includes a spraying area and a shielding area, including the following steps:

[0009] (1) Remove oil and other contaminants from product parts;

[0010] (2) installing a metal shielding fixture to a protruding portion of the product component, with a portion of the metal shielding fixture being located above the first region;

[0011] (3) Use tape to mask the sides, surfaces, and areas of the metal masking fixture that do not require spraying.

[0012] (4) Sandblasting the spraying area;

[0013] (5) Remove the tape covering the side of the metal masking fixture;

[0014] (6) Use plasma spraying technology to make a spray area in the spray area until the required spray area thickness is reached;

[0015] (7) Machining the spraying area to the required thickness and shape;

[0016] (8) Grind the areas on the product parts where the ceramic powder adheres and where there are sharp corners and burrs.

[0017] The main feature of the spraying area production process in this case is that by masking the non-spraying area, the highly difficult range of spraying can be accurately controlled in a narrow area. At the same time, by adding a metal masking fixture, the problem of difficult removal of the tape after spraying in conventional masking and spraying processes and the presence of burrs on the edge of the spraying area are avoided.

[0018] Furthermore, the width of the spraying area is a, the width of the masking area is b, the width of the upper surface of the product component is c, the length of the metal masking fixture is greater than c, and the tape can be kept away from the side of the protrusion to avoid sticking the tape to the product component, thereby causing the problem that the masking tape cannot be removed from the product component.

[0019] Furthermore, the thickness of the metal shielding jig is 10-20 mm, which can prevent the metal shielding jig from being deformed during the spraying process.

[0020] Furthermore, in step (2), a threaded hole is provided on the product component, and the metal shielding fixture is connected to the product component by bolts, thereby improving the stability of the connection between the metal shielding fixture and the product component.

[0021] Furthermore, in step (3), the thickness of the tape is 30 μm, and by adding one or more layers of tape on the side of the metal masking fixture to adjust the width a of the spraying area, the range of sandblasting and spraying can be accurately controlled.

[0022] Furthermore, in step (3), when the side of the metal masking fixture is masked with tape, the bottom of the tape is in close contact with the spraying area to prevent sand from entering from the bottom of the tape into the area that does not need sandblasting or spraying during sandblasting.

[0023] Furthermore, in step (4), the sandblasting material is 40-100 white corundum, and the surface roughness after sandblasting is 2-10 μm.

[0024] Furthermore, in step (6), the spraying material is one of aluminum oxide, yttrium oxide, etc.

[0025] Furthermore, during spraying, the power is 30-40 kW, and the gases used to generate plasma are argon and hydrogen, with a ratio of 8:1-12:1.

[0026] Furthermore, the tape is a polyimide tape, which does not leave any adhesive traces, has excellent high temperature resistance, and does not leave any residual adhesive after high-temperature peeling, and can be used for masking during painting, coating and sandblasting.

[0027] The beneficial effects of the present invention are:

[0028] 1. By adding one or more layers of tape on the side of the metal masking fixture to adjust the width a of the spraying area, the range of sandblasting and spraying can be accurately controlled;

[0029] 2. By adding a metal masking fixture, the problem of difficult removal of tape after spraying and burrs on the edge of the spraying area in conventional masking and spraying processes is avoided;

[0030] 3. When masking the side of the metal masking fixture with tape, the bottom of the tape is close to the spraying area to prevent sand from entering the area that does not need sandblasting or spraying from the bottom of the tape during sandblasting, avoiding the existence of a jagged structure on the edge of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of a product component according to an embodiment of the present invention;

[0032] Figure 2 A schematic diagram of making a spraying area on a product component according to an embodiment of the present invention;

[0033] Figure 3 A schematic diagram of installing a metal shielding fixture on a product component according to an embodiment of the present invention;

[0034] Figure 4 It is a schematic diagram of a product component and a metal masking jig coated with adhesive tape according to an embodiment of the present invention;

[0035] Figure 5 It is a cross-sectional schematic diagram of a product component and a metal shielding fixture according to an embodiment of the present invention;

[0036] Figure 6 This is a partial enlarged view of a sandblasting layer sprayed on a product component according to an embodiment of the present invention;

[0037] Figure 7 It is a schematic diagram of the spraying area on the product component according to one embodiment of the present invention.

[0038] In the figure: 1. product; 101. convex part; 102. first area; 103. side of convex part; 104. threaded hole; 2. metal masking fixture; 3. heat-resistant tape; 4. masking material; 5. sandblasting layer; 6. masking area; 7. spraying area; 8. fastening bolts. DETAILED DESCRIPTION

[0039] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0040] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the invented product is usually placed when in use, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", "third" and the like are only used to distinguish the description, and cannot be understood as indicating or implying relative importance. Terms such as "horizontal", "vertical", and "overhanging" do not mean that the components are required to be absolutely horizontal or overhanging, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", and does not mean that the structure must be completely horizontal, but can be slightly tilted.

[0041] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection, it can be a mechanical connection, it can be an electrical connection, it can be a direct connection, it can be indirectly connected through an intermediate medium, and it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0042] In this embodiment, a process for making a coating on a product surface is provided. The product comprises a first region and a convex portion. The convex portion is arranged along a first direction (attached Figure 4 The first area includes a spraying area and a shielding area, and comprises the following steps:

[0043] (1) Removing oil stains and other contaminants from the product 1; in this step, the stains on the surface of the product 1 can be removed by beating to remove the stains, or by using a solvent cleaning method to dissolve the stains into the solvent, or a combination of the two;

[0044] (2) Install the metal shielding fixture 2 to the convex portion 101 of the product 1; Figure 3 As shown in the figure, the metal shielding jig 2 is installed on the protrusion 101 of the product 1 by using the fastening bolt 8; when only one fastening bolt 8 is provided, although the metal shielding jig 2 and the protrusion 101 can be fixed, at this time, the protrusion 101 can still rotate relative to the metal shielding jig 2 with the fastening bolt 8 as the axis. In order to avoid the mutual rotation between the metal shielding jig 2 and the protrusion 101, in this example, at least two fastening bolts 8 are provided and distributed at different positions of the metal shielding jig 2. By providing multiple fastening bolts 8, the metal shielding jig 2 and the protrusion 101 can be locked from different positions, avoiding the mutual rotation between the metal shielding jig 2 and the protrusion 101, and improving the anti-torsion performance between the two;

[0045] (3) Use heat-resistant tape 3 to mask the sides and surface of the metal masking fixture 2 and the areas on the product 1 that do not require spraying; Figure 5 and attached Figure 6 As shown, while masking is being performed, the length of area a on the first area 102 can be measured in real time, and the length of area a, that is, the area range requiring sandblasting, can be accurately guaranteed while the masking thickness is continuously increased.

[0046] (4) Sandblasting the spraying area 7; sandblasting the non-shielded position to increase the roughness. The sandblasting material is 40-100 white corundum. The surface roughness after sandblasting is 2-10 μm. The inventor has conducted many experiments and found that this sandblasting material and the roughness after sandblasting are the best for making the spraying area 7.

[0047] (5) Remove the heat-resistant tape 3 covering the side of the metal masking fixture 2; since the side 103 of the protrusion is not covered by the heat-resistant tape 3, the heat-resistant tape 3 does not need to be removed after spraying, so the edge of the spraying area will be very neat, which also solves the problem of the heat-resistant tape 3 being unable to be removed due to masking the heat-resistant tape 3.

[0048] (6) Using plasma spraying technology, a spraying area 7 is formed in the first region 102 until the required thickness of the spraying area 7 is reached; the spraying material is one of aluminum oxide, yttrium oxide, etc., and the plasma spraying process is used for spraying. During the spraying, the power is 30-40 kW, and the gas used to generate the plasma is argon and hydrogen, and the ratio thereof is 8:1-12:1.

[0049] (7) machining the spraying area 7 to the required thickness and shape;

[0050] (8) Grind the areas on product 1 where ceramic powder adheres and where there are sharp corners and burrs. After thermal spraying, a small amount of ceramic powder will adhere to the areas of the product that do not need thermal spraying (i.e., areas with sharp corners and burrs). Figure 6 However, since this area is masked during the sandblasting process, it is not sandblasted, and the surface roughness of the product is low. The roughness of the original product surface is maintained, and the bonding strength between the ceramic powder and the product is low. The adhered ceramic powder can be easily removed by grinding.

[0051] The main feature of the process for making the spraying area 7 in this case is that by masking the non-spraying area with the heat-resistant tape 3, it is possible to achieve the highly difficult and precise control of the range of the spraying in a narrow area. At the same time, by adding the metal masking fixture 2, the problem of the heat-resistant tape 3 being difficult to remove after spraying in the conventional masking and spraying process and the presence of burrs on the edge of the spraying area 7 are avoided.

[0052] See attached Figure 6 and attached Figure 7 In some embodiments, the first area is shielded by the shielding object and the metal shielding fixture as the shielding area 6, the first area is not shielded by the shielding object as the spraying area 7, the width of the spraying area 7 is a, the width of the shielding area is b, the length of the convex portion is c, and a portion of the metal shielding fixture 2 is located above the first area. A portion of the metal shielding fixture 2 is located above the first area so that when the heat-resistant tape 3 is pasted on the side of the metal shielding fixture 2 for masking, the heat-resistant tape 3 can be away from the side of the convex portion 103, so as to avoid pasting the heat-resistant tape 3 on the product 1, thereby solving the problem that the masking heat-resistant tape 3 cannot be removed from the product 1.

[0053] In some embodiments, the thickness of the metal shielding jig 2 is 10-20 mm to ensure that the metal shielding jig 2 has sufficient thickness, so that the heat-resistant tape 3 can be attached to the side of the metal shielding jig 2 in the subsequent steps, and the metal shielding jig 2 can be prevented from being deformed during the spraying process. At the same time, the surface roughness of the metal shielding jig 2 is below 0.5 μm, and the surface of the metal shielding jig 2 is relatively smooth. When the spraying area 7 is sprayed, the bonding strength between the spraying material and the metal shielding jig 2 is low, and it is not easy to adhere to the metal shielding jig 2. The ceramic powder can be removed by simple grinding at a later stage.

[0054] See attached Figure 1 In some embodiments, in step (2), a threaded hole 104 is provided on the product 1, and a through hole is correspondingly provided on the metal shielding jig 2. The metal shielding jig 2 is connected to the product 1 by bolts. After the fastening bolt 8 passes through the metal shielding jig 2, it continues to be screwed into the threaded hole 104 on the product 1. The fastening bolt 8 can be used in conjunction with a spring washer to improve the stability of the connection between the metal shielding jig 2 and the product 1.

[0055] At least two fastening bolts 8 are provided and distributed at different positions of the metal shielding fixture 2. By providing multiple fastening bolts 8, the metal shielding fixture 2 and the protrusion 101 can be locked from different positions, thereby preventing the metal shielding fixture 2 and the protrusion 101 from rotating relative to each other and improving the anti-torsion performance between the two.

[0056] See attached Figure 5 To Attachment Figure 6 In some embodiments, in step (3), the thickness of the heat-resistant tape 3 is 30 μm. By adding one or more layers of heat-resistant tape 3 on the side of the metal masking jig 2, the width a of the spraying area 7 is adjusted. In order to accurately control the unmasked range at the target value a, when the heat-resistant tape 3 is attached to the side of the metal masking jig 2, the number of sheets of heat-resistant tape 3 or heat-resistant tape 3 of different thicknesses can be increased, so that the range of sandblasting and spraying can be accurately controlled.

[0057] See attached Figure 6 In some embodiments, in step (3), when the side of the metal masking fixture 2 is masked with the heat-resistant tape 3, the bottom of the heat-resistant tape 3 is in close contact with the spraying area 7 to prevent sand from entering the area that does not need sandblasting or spraying from the bottom of the heat-resistant tape 3 during sandblasting.

[0058] In some embodiments, in step (4), the non-shielded position is sandblasted to increase the roughness, the sandblasting material is 40-100 white corundum, and the surface roughness after sandblasting is 2-10 μm. The inventors have conducted multiple experiments and found that this sandblasting material and the roughness after sandblasting are the best for making the spraying area 7.

[0059] In some embodiments, in step (6), the spraying material is one of aluminum oxide, yttrium oxide, etc., and the spraying is performed using a plasma spraying process. During the spraying, the power is 30-40 kW, and the gas used to generate the plasma is argon and hydrogen, and the ratio thereof is 8:1-12:1.

[0060] In some embodiments, the heat-resistant tape 3 is a polyimide tape, or other adhesive tape with fixed heat resistance and other properties, suitable for spray painting, decoration and electronic industries. The curing adhesive on the heat-resistant tape 3 provides excellent solvent resistance and high temperature resistance, and does not leave any adhesive traces, has excellent high temperature resistance, and does not leave any residual adhesive after high temperature peeling, and can be used for shielding during spray painting, coating and sandblasting.

[0061] In step (7), after spraying, a small amount of ceramic powder will adhere to the area of ​​the product that does not need spraying (i.e. Figure 6However, since this area is masked during the sandblasting process, it is not sandblasted, and the surface roughness of the product is low. The roughness of the original product surface is maintained, and the bonding strength between the ceramic powder and the product is low. The adhered ceramic powder can be easily removed by grinding.

[0062] In step (8), the areas on the product 1 that are adhered to the ceramic powder and the areas with sharp corners and burrs are ground, and the sprayed areas are machined to machine the coating to the required thickness.

[0063] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for making a coating on a product surface, wherein the product comprises a first region and a convex portion, wherein the convex portion is higher than the first region along a first direction, wherein: The process comprises the following steps: (1) installing a metal shielding fixture on the protrusion, wherein a portion of the metal shielding fixture is located above the first area; (2) shielding the side of the metal shielding jig with a shielding object, wherein the bottom of the shielding object is in close contact with the first area, so as to form a spraying area and a shielding area on the first area; (3) sandblasting the spraying area; (4) Remove the tape covering the side of the metal masking fixture; (5) performing a spraying process in the spraying area to form the coating, The thickness of the metal shielding fixture is 10-20 mm, and the surface roughness of the metal shielding fixture is below 0.5 μm.

2. The process for making a coating on a product surface according to claim 1, characterized in that: The width of the spraying area is a, the masking material is a tape, the thickness of the tape is 30 μm, and the width a of the spraying area is adjusted by adding one or more layers of tape on the side of the metal masking fixture.

3. The process for making a coating on a product surface according to claim 1, characterized in that: Before step (1), the method further includes removing oil pollution on the first area.

4. The process for making a coating on a product surface according to claim 1, characterized in that: In step (1), the metal shielding fixture is connected to the product by bolts.

5. The process for making a coating on a product surface according to claim 1, characterized in that: In step (3), the blasting material used for blasting the spraying area is 40-100 white corundum, and the surface roughness after blasting is 2-10 μm.

6. The process for making a coating on a product surface according to claim 1, characterized in that: The spraying material is one of aluminum oxide and yttrium oxide.

7. The process for making a coating on a product surface according to claim 6, characterized in that: The spraying is plasma spraying, the spraying power is 30-40 kW, and the gases used to generate plasma are argon and hydrogen, with a ratio of 8:1-12:1.