An iron-based electrode material and its preparation method and application
By uniformly distributing iron particles on the carbon material skeleton, the problem of hydrogen evolution passivation of the iron-nickel battery anode material is solved, the activity and utilization rate of the electrode material are improved, higher conductivity and cycle stability are achieved, and it is suitable for large-scale scale production.
Patent Information
- Application Number
- CN202311709733.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-12
AI Technical Summary
Existing iron-nickel battery anode materials suffer from hydrogen evolution passivation during the charge and discharge process, resulting in reduced utilization and conductivity and affecting cycle stability.
Using carbon material as the skeleton, evenly distributing iron element particles on it, using iron source, carbon source, metal salt and acid solution to mix and dissolve, and then undergo high-temperature sintering and reduction treatment to form an iron base with a two-dimensional nanosheet structure. Electrode materials.
It significantly improves the activity and utilization of the anode material, enhances the conductivity, simplifies the preparation process, reduces the cost, is suitable for mass production, and improves the cycle stability of the battery.
Smart Images

Figure CN117878299B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to an iron-based electrode material and a preparation method and application thereof. Background Art
[0002] Iron-nickel batteries have attracted more and more attention due to their high conductivity, high efficiency, high safety and low cost. Moreover, iron-nickel batteries have the characteristics of high theoretical capacity, sturdiness, mature production technology, recyclability and eco-friendly, so they are considered more suitable for use as energy storage devices.
[0003] Among them, iron in different valence states is the main reactant of the anode material. However, in actual use, the iron anode has problems such as self-discharge, hydrogen evolution passivation during the charge and discharge process, relatively low energy density, and low utilization rate. At present, hydrogen evolution passivation in commercial iron-nickel batteries leads to a decrease in utilization and conductivity, and the cycle stability is also greatly affected, which greatly hinders the development of iron-nickel batteries.
[0004] Therefore, how to reduce the hydrogen evolution passivation phenomenon of the anode material and improve the conductivity and utilization rate of the anode material is a technical problem that needs to be solved urgently. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes an iron-based electrode material and a preparation method and application thereof. The iron-based electrode material of the present invention uses carbon material as a skeleton to grow particles containing iron elements, and its activity as an anode material is significantly higher than that of traditional commercial iron-nickel battery anode materials. In addition, the preparation method of the iron-based electrode material of the present invention is simple and convenient, and can increase the utilization rate of the anode material.
[0006] A first aspect of the present invention provides an iron-based electrode material.
[0007] Specifically, an iron-based electrode material includes a carbon material skeleton and iron-containing particles supported on the carbon material skeleton.
[0008] Preferably, the iron-containing particles account for 50-95% of the total weight of the iron-based electrode material.
[0009] Preferably, the iron-based electrode material has a two-dimensional nanosheet structure.
[0010] Preferably, the chemical composition of the iron-containing particles is metallic iron or iron nitride.
[0011] Preferably, the iron-based electrode material does not contain acid and salt.
[0012] A second aspect of the present invention provides a method for preparing an iron-based electrode material.
[0013] Specifically, a method for preparing an iron-based electrode material comprises the following steps:
[0014] S1, mixing a carbon source and an iron source in a solvent to obtain a mixed solution;
[0015] S2, adding the metal salt and the acid solution into the mixed solution of step S1 and mixing them to obtain a mixture, and drying the mixture to obtain a powder mixture;
[0016] S3, heat-treating the mixture in step S2 in an inert atmosphere, washing and drying, and placing the obtained substance in a reducing atmosphere for reduction treatment to obtain the iron-based electrode material.
[0017] Preferably, in step S1, the solvent includes water.
[0018] Preferably, in step S1, the mass ratio of the carbon source to the iron source is 8:(4-200), and more preferably 8:(6-150).
[0019] Preferably, in step S1, the carbon source includes at least one of glucose, soluble starch and polyvinyl pyrrolidone.
[0020] Preferably, in step S1, the iron source includes at least one of ferric chloride hexahydrate, ferrous sulfate tetrahydrate, and ferrous sulfate heptahydrate.
[0021] Preferably, in step S1, the metal salt includes at least one of sodium chloride and potassium chloride.
[0022] Preferably, in step S2, the drying is freeze-drying.
[0023] Preferably, in step S2, the acid solution includes at least one of sulfuric acid solution, hydrochloric acid, and acetic acid solution.
[0024] Preferably, the mass ratio of the carbon source to the acid solution is 10:(1-20), more preferably 10:(1-10).
[0025] Preferably, in step S3, the temperature of the heat treatment is 600-700°C, more preferably 680-700°C.
[0026] Preferably, in step S3, the heat treatment time is 30-300 min, more preferably 40-250 min.
[0027] Preferably, in step S3, the inert atmosphere includes at least one of argon and nitrogen.
[0028] Preferably, in step S3, the reducing atmosphere includes at least one of hydrogen, carbon monoxide and ammonia.
[0029] Preferably, in step S3, the reduction treatment is performed at a temperature of 500-900° C. and for a time of 30-300 min.
[0030] More preferably, the reduction treatment is carried out at a temperature of 550-850° C. and for a time of 40-250 min.
[0031] A third aspect of the present invention provides the use of the above-mentioned iron-based electrode material.
[0032] Specifically, an anode material includes the above-mentioned iron-based electrode material.
[0033] An iron-nickel battery comprises the above-mentioned anode material.
[0034] Preferably, the iron-nickel battery is an alkaline iron-nickel battery.
[0035] The application of the above iron-based electrode material in the oxidation reaction of the anode material of the iron-nickel battery in an alkaline environment.
[0036] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0037] (1) The iron-based electrode material of the present invention uses carbon as a skeleton to grow particles containing iron elements, and its activity as an anode material is significantly higher than that of traditional commercial iron-nickel battery anode materials. In addition, the preparation method of the iron-based electrode material of the present invention is simple and convenient, which can increase the utilization rate of the anode material.
[0038] (2) The present invention obtains iron-containing particles grown on a carbon skeleton by mixing and dissolving an iron source, a carbon source, a metal salt and an acid solution, and then subjecting the mixture to a heat treatment (high-temperature sintering) and a reduction treatment. The solution formed by using iron metal salt, glucose and metal salt can not only make the iron-containing particles evenly distributed on the carbon skeleton, but also significantly improve the coupling between the active substance and the carbon element in the anode material. At the same time, the effective combination of the active substance and the carbon element can also significantly improve the utilization rate of the active substance and the conductivity during the reaction process.
[0039] (3) The preparation method of the present invention is simple and convenient, the conditions are controllable, the efficiency is high, the utilization rate of active substances is high, the stable metal salt can be recycled and reused, the cost is low, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic flow chart of the method for preparing the iron-based electrode material based on the carbon material skeleton of the present invention;
[0041] Figure 2 This is a scanning electron microscope image of the ammonia-reduced active material prepared in Example 1;
[0042] Figure 3 This is a scanning electron microscope image of the ammonia-reduced active material prepared in Example 1;
[0043] Figure 4 This is a scanning electron microscope image of the hydrogen-reduced active material prepared in Example 2;
[0044] Figure 5 This is a scanning electron microscope image of the hydrogen-reduced active material prepared in Example 2;
[0045] Figure 6 Comparison diagram of cyclic voltammetry curves of Example 1, Example 2, Comparative Example 1, and Comparative Example 2 in 4M KOH+0.2M LiOH electrolyte;
[0046] Figure 7 It is a comparison diagram of constant current charge and discharge curves of Example 1, Example 2, Comparative Example 1, and Comparative Example 2 in 4M KOH+0.2M LiOH electrolyte respectively. DETAILED DESCRIPTION
[0047] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0048] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0049] like Figure 1 As shown, the method for preparing the iron-based electrode material provided by the present invention comprises the following steps:
[0050] S1. mixing a carbon source and an iron source in water to obtain a mixed solution;
[0051] S2, adding the metal salt and the acid solution to the mixed solution and mixing to obtain a mixture; freeze-drying the mixture to obtain a powder mixture;
[0052] S3. After treating the obtained powder mixture at high temperature in an inert atmosphere, washing and drying, the obtained substance is placed in a reducing atmosphere for reduction treatment to obtain an iron-based electrode material; the iron-based electrode material does not contain acid and salt.
[0053] Example 1
[0054] An iron-based electrode material comprises a carbon material skeleton and iron-containing particles loaded on the carbon material skeleton.
[0055] A method for preparing an iron-based electrode material comprises the following steps:
[0056] S1. Add 1.62 g of ferric chloride hexahydrate and 2.16 g of glucose to 100 ml of deionized water, stir until dissolved to obtain a mixed solution, then add 10 g of sodium chloride and 85 μl of concentrated sulfuric acid solution (the mass fraction of the concentrated sulfuric acid solution is 97%), stir for 2 hours to obtain a mixture, and freeze-dry overnight to obtain a powder mixture;
[0057] S2. After placing the obtained powder mixture in a tube furnace and heat treating it at 700° C. for 1 hour under an argon environment, the product is washed (washed with deionized water 5 times) until there is no sodium chloride, and then the obtained material is dried for standby use;
[0058] S3, placing the substance obtained in step S2 in an ammonia environment at 700° C. for reaction for 3 hours to obtain an iron-based electrode material.
[0059] Example 2
[0060] An iron-based electrode material comprises a carbon material skeleton and iron-containing particles loaded on the carbon material skeleton.
[0061] A method for preparing an iron-based electrode material comprises the following steps:
[0062] S1. Add 1.62 g of ferric chloride hexahydrate and 2.16 g of glucose to 100 ml of deionized water, stir until dissolved to obtain a mixed solution, then add 10 g of sodium chloride and 85 μl of concentrated sulfuric acid solution (the mass fraction of the concentrated sulfuric acid solution is 97%), stir for 2 hours to obtain a mixture, and freeze-dry overnight to obtain a powder mixture;
[0063] S2. After placing the obtained powder mixture in a tube furnace and heat treating it at 700° C. for 1 hour under an argon environment, the product is washed (washed with deionized water 5 times) until there is no sodium chloride, and then the obtained material is dried for standby use;
[0064] S3. Place the substance obtained in step S2 in a hydrogen environment at 700° C. for reaction for 3 hours to obtain an iron-based electrode material.
[0065] Comparative Example 1 (the difference from Example 1 is that carbon material is physically added for mixing)
[0066] This comparative example provides a method for preparing a conventional iron oxide anode, comprising the following steps:
[0067] S1, directly purchase commercial ferroferric oxide powder;
[0068] S2. Mix ferroferric oxide powder, superconducting carbon black and polyvinylidene fluoride in a weight ratio of 90:6:4, and then mix with N-methylpyrrolidone to obtain a solid concentration of 20 mg mL -1The mixed slurry is coated on the electrode and dried to obtain a conventional iron oxide anode.
[0069] Comparative Example 2 (the difference from Example 1 is that a different skeleton is used)
[0070] This comparative example provides a method for preparing an iron-based material, comprising the following steps:
[0071] S1. Ferrocene and thiophene were mixed in a mass ratio of 95:5 as a catalyst, 80% ethanol and 20% acetone were used as carbon sources (80% of the mass of the carbon source was ethanol and 20% of the mass of acetone), and a three-dimensional carbon nanotube network was prepared at 1000° C. in an atmosphere of 95% argon and 5% hydrogen (95% of the volume of the atmosphere was argon and 5% of the volume was hydrogen);
[0072] S2. Mix ferroferric oxide powder and polyvinylidene fluoride in a weight ratio of 95:5, and then mix with N-methylpyrrolidone to obtain a solid concentration of 20 mg mL -1 The mixed slurry is coated on the above-mentioned carbon nanotube three-dimensional network and dried to obtain an iron-based material.
[0073] Related characteristics test
[0074] 1. Electron microscope scanning analysis of iron-based electrode materials:
[0075] The iron-based electrode materials prepared in Example 1 and Example 2 were subjected to electron microscope scanning analysis. The scanning electron microscope photo of the iron-based electrode material prepared in Example 1 is as follows: Figure 2 , Figure 3 As shown. Figure 2 and Figure 3 It can be clearly seen that the iron-based electrode material prepared in Example 1 has a two-dimensional nanosheet structure and a large surface area, and the iron particles are evenly distributed on the two-dimensional nanosheet. The scanning electron microscope photos of the iron-based electrode material prepared in Example 2 are as follows: Figure 4 , Figure 5 As shown, the iron particles loaded in the obtained iron-based electrode material are still evenly distributed on the two-dimensional nanosheets, and the particles are reduced. It can be seen that dissolving in aqueous solution followed by drying and sintering is a key step in preparing the two-dimensional nanosheet structure.
[0076] 2. Electrochemical performance test of iron-based electrode materials:
[0077] The iron-based electrode materials prepared in Example 1 and Example 2, the conventional iron oxide anode prepared in Comparative Example 1, and the iron-based material in Comparative Example 2 were loaded on carbon cloth, respectively, and then electrochemically tested in 4M KOH+0.2M LiOH electrolyte ("M" means "mol / L"), respectively.
[0078] The electrochemical test results are as follows Figure 6 , Figure 7 As shown by Figure 6 It can be seen that: under the condition of the same iron element loading on the electrode, the iron-based electrode materials based on the carbon skeleton prepared in Example 1 and Example 2 both have relatively obvious redox peaks, so the iron-based electrode materials based on the carbon skeleton have good polarization phenomenon in the cyclic voltammetry test. At the same time, compared with Comparative Example 1 and Comparative Example 2, their cyclic voltammetry curve areas are obviously larger. Figure 7 It can be seen that: when the iron element loading on the electrode is the same, the iron-based electrode materials based on the carbon material skeleton prepared in Example 1 and Example 2 have good capacitance in the constant current charge and discharge test, and the capacitance of Example 1 and Example 2 is also significantly improved compared with Comparative Example 1 and Comparative Example 2. Therefore, in summary, Example 1 and Example 2 have more superior electrochemical performance than Comparative Example 1 and Comparative Example 2.
[0079] The above electron microscope scanning and electrochemical performance test data show that the iron-based electrode material based on the carbon material skeleton prepared by the present invention has a two-dimensional nano-sheet structure and a uniformly distributed particle structure, and has excellent polarization performance and capacitance. In addition, the iron-based electrode material based on the carbon material skeleton prepared by the present invention has a stable structure and performance, low cost, and can be mass-produced, effectively overcoming the problems of hydrogen evolution passivation and cumbersome laboratory preparation process and poor binding of the existing commercial iron-nickel battery anode, and can replace commercial iron electrodes for use in alkaline iron-nickel batteries.
[0080] The preferred embodiments of the present invention are specifically described above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. An iron-based electrode material for an iron-nickel battery, characterized in that: It includes a carbon material skeleton and iron-containing particles supported on the carbon material skeleton; The method for preparing the iron-based electrode material comprises the following steps: S1, mixing a carbon source and an iron source in a solvent to obtain a mixed solution; S2, adding the metal salt and the acid solution into the mixed solution of step S1 and mixing them to obtain a mixture, and drying the mixture to obtain a powder mixture; S3, heat-treating the mixture in step S2 in an inert atmosphere, then washing and drying, and placing the obtained substance in a reducing atmosphere for reduction treatment to obtain the iron-based electrode material; In step S1, the carbon source includes at least one of glucose, soluble starch, and polyvinyl pyrrolidone; and / or the iron source includes at least one of ferric chloride hexahydrate, ferrous sulfate tetrahydrate, and ferrous sulfate heptahydrate; and / or the metal salt includes at least one of sodium chloride and potassium chloride; In step S2, the acid solution includes at least one of sulfuric acid solution, hydrochloric acid, and acetic acid solution; The reducing atmosphere includes at least one of hydrogen, carbon monoxide and ammonia; the temperature of the reduction treatment is 500-900° C. and the time is 30-300 minutes.
2. The iron-based electrode material according to claim 1, characterized in that The iron-containing particles account for 50-95% of the total weight of the iron-based electrode material.
3. The iron-based electrode material according to claim 1, characterized in that The iron-based electrode material has a two-dimensional nanosheet structure.
4. The method for preparing the iron-based electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, mixing a carbon source and an iron source in a solvent to obtain a mixed solution; S2, adding the metal salt and the acid solution into the mixed solution of step S1 and mixing them to obtain a mixture, and drying the mixture to obtain a powder mixture; S3, heat-treating the mixture in step S2 in an inert atmosphere, then washing and drying, and placing the obtained substance in a reducing atmosphere for reduction treatment to obtain the iron-based electrode material; In step S1, the carbon source includes at least one of glucose, soluble starch, and polyvinyl pyrrolidone; and / or the iron source includes at least one of ferric chloride hexahydrate, ferrous sulfate tetrahydrate, and ferrous sulfate heptahydrate; and / or the metal salt includes at least one of sodium chloride and potassium chloride; In step S2, the acid solution includes at least one of sulfuric acid solution, hydrochloric acid, and acetic acid solution; The reducing atmosphere includes at least one of hydrogen, carbon monoxide and ammonia; the temperature of the reduction treatment is 500-900° C. and the time is 30-300 minutes.
5. The preparation method according to claim 4, characterized in that: In step S1, the solvent includes water; and / or, in step S1, the mass ratio of the carbon source to the iron source is 8:(4-200).
6. The preparation method according to claim 4, characterized in that: In step S2, the mass ratio of the carbon source to the acid solution is 10:(1-20).
7. The preparation method according to claim 4, characterized in that: In step S3, the temperature of the heat treatment is 600-700° C.; and / or the time of the heat treatment is 30-300 min.
8. An anode material, characterized in that: The invention comprises the iron-based electrode material for the iron-nickel battery according to any one of claims 1 to 3.
9. An iron-nickel battery, characterized in that: Comprising the anode material according to claim 8.
Citation Information
Patent Citations
Fe3O4 / C composite material, its preparation method and its application in lithium ion battery
CN103825019A
Preparation method of nickel iron battery anode material
CN105161685A
Composite negative electrode material and preparation method and application thereof
CN111785947A