Self-healing inorganic concrete proliferating waterproofing agent, its preparation method and preparation apparatus
By using self-healing inorganic concrete proliferation waterproofing agent in concrete, using components such as silane coupling agent and nano-mineral powder to fill the cracks, forming a high-durability reticulum structure, the low anti-seepage performance and self-healing of concrete in the prior art are solved. Due to the long-term problem, efficient crack sealing and continuous repair have been achieved, which significantly improves the seepage resistance and durability of concrete.
Patent Information
- Application Number
- CN202410084158.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-01-19
AI Technical Summary
The existing self-healing admixtures for concrete cracks have problems such as low efficiency, high cost, complex process and long self-healing time in improving concrete seepage resistance, and cannot effectively extend the service life and durability of concrete.
Self-healing inorganic concrete proliferation waterproofing agent, including silane coupling agent, reaction accelerator, nano-mineral powder, fluorosilicate and basalt fibers, are used to fill the cracks through coupling reaction and crystallization precipitation to form a high-durability reticulum structure. , improve the compactness and compressive strength of concrete, and provide silicate ions and calcium ions through fluorosilicate and nano-mineral powder to promote long-term reactions.
It achieves rapid sealing, continuous repair and high reliability self-healing effects of concrete, significantly improves the anti-seepage performance, durability and density, and extends the service life of concrete.
Smart Images

Figure CN117886545B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of concrete admixtures, and more specifically, to a self-healing inorganic concrete proliferation waterproofing agent, a preparation method thereof, and a preparation device thereof. Background Art
[0002] Concrete is a porous and brittle material, which is widely used in the field of basic construction. Due to the influence of external environmental factors, concrete is prone to cracks. Water seepage in the cracks will reduce the strength of concrete, aggravate the chemical erosion of concrete, steel corrosion and alkali-aggregate reaction, and seriously reduce the durability of concrete structures, which not only causes serious losses to national property and economy, but also threatens people's lives and safety.
[0003] In the prior art, in order to improve the comprehensive anti-seepage performance of concrete and enhance the durability of concrete structures, crack self-healing admixtures are usually added to concrete to improve the comprehensive anti-seepage performance of concrete. The principles adopted by common concrete crack self-healing admixtures include: microbial self-healing, microcapsule self-healing and osmotic crystallization self-healing. However, the microbial self-healing method cannot improve the compactness of concrete itself, and it takes a long time for the microorganisms to have life activities to block the cracks. The comprehensive anti-seepage performance is not good, and the microorganisms used need to be cultivated and are difficult to produce; in the microcapsule self-healing method, the microcapsules are difficult to rupture and the active substances are not fully released, so that the comprehensive anti-seepage performance of the concrete cannot be guaranteed, and the microcapsule production process is complicated, the cost is high, and the construction is difficult; the self-healing repair time of the osmotic crystallization self-healing method is long, the repair effect is limited, and the comprehensive anti-seepage performance is poor.
[0004] In response to the above-mentioned related technologies, the present application discloses a self-healing inorganic concrete proliferation waterproofing agent, which can effectively increase density, waterproof, and self-heal cracks, and extend the use effect and service life of concrete materials. Summary of the invention
[0005] In order to improve the crack self-healing effect of concrete admixtures, the present application provides a self-healing inorganic concrete proliferation waterproofing agent, a preparation method and a preparation device thereof.
[0006] In the first aspect, the present application provides a self-healing inorganic concrete proliferation waterproofing agent, which adopts the following technical solution: a self-healing inorganic concrete proliferation waterproofing agent, comprising the following components in parts by weight:
[0007] Silane coupling agent 10-30 parts,
[0008] 2-6 parts of reaction accelerator,
[0009] 20-40 parts of nano mineral powder,
[0010] Fluorosilicate 7-10 parts,
[0011] Basalt fiber 0-3 parts,
[0012] Rust inhibitor 0-4 parts;
[0013] The reaction accelerator is anhydrous sodium sulfate.
[0014] By adopting the above technical solution, the reaction accelerator can further stimulate the cement particles in the concrete that are not fully hydrated to continue hydration. The hydration products react with the SO4 in the reaction accelerator. 2- The concrete contains more Ca 2+ SO4 in the reaction accelerator 2 - The reaction generates crystalline precipitation to further fill the cracks, so that the concrete cracks are quickly sealed, reducing the penetration of water into the concrete, increasing the density of the concrete, compensating for the erosion damage of the cracks, and improving the compressive strength of the concrete;
[0015] On the one hand, the silane coupling agent can react with concrete to generate siloxane polymers, siloxane substances and a large number of calcium silicate hydrate (CSH) crystals. The CSH crystals cooperate with the Aft crystals, overlap and enrich on the inside of the crack section, fill and seal the cracks again, and the generated CSH crystals are of the same material as the concrete itself, with high durability. On the other hand, the silane coupling agent forms a mesh film on the surface of the concrete, improves the internal structure of the concrete, and compensates for the damage of the concrete cracks. The physical action and chemical changes of the silane coupling agent work together to make the concrete crack self-healing with high reliability and high durability, and improve the comprehensive anti-seepage performance of the concrete.
[0016] Basalt fiber shares tensile stress, improves the tensile performance of concrete, effectively limits the crack width of the stress-free zone of concrete, and inhibits the development trend of cracks. As an inorganic high-performance fiber, basalt fiber is long-lasting and effective with excellent durability. At the same time, basalt fiber can act as the nucleus of CSH crystals, Aft crystals, etc., promote the formation of crystals, and further enhance the self-healing performance of concrete.
[0017] During the crack repair process, fluorosilicate and nano-mineral powder provide abundant silicate ions and calcium ions, making the reaction process between the reaction accelerator, silane coupling agent and concrete long-lasting and effective, further improving the durability of the concrete self-healing proliferation waterproofing agent;
[0018] To sum up, the raw materials of the self-healing inorganic concrete proliferation waterproofing agent of the present application cooperate with each other, which can play an excellent concrete self-healing effect in both rapid water blocking in the early stage of cracking and seepage and continuous repair in the later stage, and has long-term effectiveness, greatly improving the durability, waterproofness and density of concrete.
[0019] Preferably, the silane coupling agent is an aminosilane coupling agent.
[0020] Preferably, the fluorosilicate is selected from potassium fluorosilicate, sodium fluorosilicate or a combination of both.
[0021] By adopting the above technical scheme, fluorosilicate mainly plays the role of promoting the solidification of concrete and improving its corrosion resistance. Fluorosilicate can effectively prolong the setting time of concrete, enrich the unhydrated silicate ions in concrete, and make the concrete structure have good working performance, impermeability and durability.
[0022] Preferably, the nano mineral powder is nano silicon dioxide, nano calcium carbonate and nano clay in a mass ratio of 1:(0.8-1.2):(0.6-1.3).
[0023] By adopting the above technical solution, nano mineral powder can provide sufficient and rich inorganic silicon ions and calcium ions with stable chemical properties and low cost.
[0024] Preferably, the basalt fiber has a fiber length of 12-18 mm and a tensile strength of 3000-4800 MPa.
[0025] By adopting the above technical solution, the tensile strength of basalt fiber can be controlled to 3000-4800MPa, which can effectively reduce the amount of early cracks in concrete and reduce the crack width, thereby improving the early cracking resistance of concrete.
[0026] Preferably, the rust inhibitor is diammine silver hydroxide.
[0027] By adopting the above technical solution, silver diammine hydroxide can reduce the possibility of steel bar corrosion in concrete and ensure the application stability of concrete materials.
[0028] In a second aspect, the present application provides a method for preparing a self-healing inorganic concrete proliferation waterproofing agent, using the following technical solution:
[0029] A method for preparing a self-healing inorganic concrete proliferation waterproofing agent comprises the following steps:
[0030] According to the formula, silane coupling agent, fluorosilicate, nano mineral powder, basalt fiber, reaction accelerator and rust inhibitor are fully mixed and dispersed to obtain a self-healing inorganic concrete proliferation waterproofing agent.
[0031] By adopting the above technical solution, the various components cooperate with each other to give the concrete excellent self-healing properties, thereby improving the long-term durability, density, and anti-seepage and waterproof properties of the concrete.
[0032] In a third aspect, the present application provides a stirring device for use in the preparation method of the above-mentioned self-healing inorganic concrete proliferation waterproofing agent, which adopts the following technical solution:
[0033] A preparation device for a self-healing inorganic concrete proliferation waterproofing agent comprises a frame mechanism and a stirring mechanism, wherein the stirring mechanism comprises a stirring member and a driving member, wherein the stirring member is rotatably arranged on the frame mechanism, the driving member is mounted on the frame mechanism and connected to the stirring member, and the driving member is used to drive the stirring member to rotate.
[0034] By adopting the above technical solution, the raw materials are put into the stirring member, and the driving member drives the stirring member to rotate, so that the stirring member can fully stir the raw materials, which is conducive to fully mixing and dispersing the raw material components.
[0035] Preferably, the frame mechanism includes a supporting base, a supporting column arranged on the supporting base, and a traction arm connected to the supporting column; the stirring element includes a mixing tank, a central shaft and a spiral blade, one end of the central shaft is rotatably connected to the supporting column, and the other end is rotatably connected to the traction arm; the mixing tank is sleeved on the central shaft and rotates coaxially with the central shaft, and one end of the mixing tank close to the supporting column is connected to the central shaft, and the other end is open for loading or unloading; the spiral blade is arranged on the central shaft and is located in the inner cavity of the mixing tank; the driving member is connected to the outer wall of the mixing tank to drive the mixing tank to rotate.
[0036] The adoption of the above technical solution is conducive to improving the installation stability and rotation stability of the mixing tank and the central shaft, so that each raw material component can be stirred stably and fully.
[0037] Preferably, a plurality of stirring columns are evenly arranged on the inner wall of the mixing tube.
[0038] By adopting the above technical solution, the uniformity of dispersion of each raw material component is further improved.
[0039] Preferably, the driving member includes a driving motor, a driving gear, a gear mounting seat and a mounting gear ring, the driving motor and the gear mounting seat are both arranged on the supporting base, the driving gear is mounted on the gear mounting seat, and the output end of the driving motor is connected to the driving gear, and the mounting gear ring is sleeved on the outer wall of the mixing tank and meshed with the driving gear.
[0040] By adopting the above technical solution, the driving motor drives the driving gear to rotate, and then drives the stirring tank to rotate through the installed gear ring, and the raw material components are fully stirred by the spiral blades.
[0041] In summary, this application has the following beneficial effects:
[0042] 1. In this application, the reaction accelerator further stimulates the cement particles in the concrete that are not fully hydrated to continue hydration, and the hydration products react with the SO4 in the reaction accelerator. 2- Gypsum and a large number of needle-shaped calcium sulfide crystals are generated to fill the cracks. At the same time, the concrete contains more Ca 2+ SO4 in the reaction accelerator 2- The reaction generates crystalline precipitation to further fill the cracks, so that the concrete cracks are quickly blocked, reducing the penetration of water into the concrete, increasing the compactness of the concrete, compensating for the damage caused by crack erosion, and improving the compressive strength of the concrete; a coupling reaction occurs between the silane coupling agent and the concrete to generate siloxane polymers, siloxane substances and a large number of calcium silicate hydrate (CSH) crystals, and AFt and CSH gel overlap and enrich on the inside of the crack section to fill and block the cracks again; the reaction accelerator cooperates with the silane coupling agent to achieve excellent self-healing effects in both the early stage of concrete cracking and water seepage and the later stage of continuous repair;
[0043] 2. This application improves the tensile strength of concrete by adding basalt fiber, effectively inhibits the development trend of cracks, and basalt fiber, silane coupling agent and reaction accelerator can be used as the nucleus point for crystal formation, thereby enhancing the self-healing performance of concrete;
[0044] 3. In the process of crack repair, the present application adds fluorosilicate and nano-mineral powder to provide surplus silicate ions and calcium ions, so that the reaction process between the silane coupling agent and the concrete is long-lasting and effective. At the same time, the basalt fiber has a long service life, which can make the concrete cracks self-healing to achieve high reliability and high durability;
[0045] 4. The raw material cost of the self-healing inorganic concrete proliferation waterproofing agent of the present application is low, it is convenient and easy to obtain, and the preparation method consumes less energy, which is conducive to expanding the application of the self-healing inorganic concrete proliferation waterproofing agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a structural schematic diagram of a preparation device of a self-healing inorganic concrete proliferation waterproofing agent in Example 16 of the present application;
[0047] Figure 2 It is a schematic cross-sectional view in the vertical direction used to show the stirring element in Example 16 of the present application. Description of the drawings:
[0049] 1. Frame mechanism; 11. Support base; 12. Support column; 13. Towing arm; 2. Stirring mechanism; 3. Stirring element; 31. Mixing tank; 311. Inlet and outlet tank; 312. Mixing tank; 313. Stirring column; 32. Center shaft; 33. Spiral blade; 4. Driving element; 41. Driving motor; 42. Driving gear; 43. Gear mounting seat; 44. Installing gear ring. DETAILED DESCRIPTION
[0050] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of these described embodiments are only partial embodiments of the present invention, not all of them.
[0051] The following specific embodiments may be combined with each other, and the same or similar concepts or processes may not be repeated in some embodiments; and the reaction devices, monomer compounds, initiators, emulsifiers, demulsifiers, and organic solvents involved in the following embodiments are all commercially available.
[0052] The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be described in detail in some embodiments.
[0053] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.
[0054] Example
[0055] Example 1
[0056] This embodiment discloses a self-healing inorganic concrete proliferation waterproofing agent, including the following components by mass: 1 kg of silane coupling agent, 0.2 kg of reaction accelerator, 2 kg of nano mineral powder, and 0.7 kg of fluorosilicate.
[0057] In this embodiment, the silane coupling agent is silane coupling agent KH550; the reaction accelerator is anhydrous sodium sulfate; the nano mineral powder is a mixture of nano silicon dioxide, nano calcium carbonate, and nano clay in a mass ratio of 1:0.9:0.8, the nano silicon dioxide is commercially available fumed silica, the nano calcium carbonate is commercially available nano-grade calcium carbonate, and the nano clay is commercially available nano-grade calcium-based bentonite; and the fluorosilicate is potassium fluorosilicate.
[0058] The preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows:
[0059] The above-mentioned mass of silane coupling agent, anhydrous sodium sulfate, nano mineral powder and potassium fluorosilicate were put into a mixer, stirred at a speed of 250 r / min for 25 minutes, and sieved to obtain a self-healing inorganic concrete proliferation waterproofing agent.
[0060] The mixer in this embodiment is a commercially available GH-5L mixer.
[0061] Example 2
[0062] The only difference between this embodiment and Embodiment 1 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2 kg of silane coupling agent, 0.2 kg of anhydrous sodium sulfate, 2 kg of nano mineral powder, and 0.7 kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0063] Example 3
[0064] The only difference between this embodiment and Example 1 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 3kg of silane coupling agent, 0.2kg of anhydrous sodium sulfate, 2kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0065] Example 4
[0066] The only difference between this embodiment and embodiment 2 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.4kg of anhydrous sodium sulfate, 2kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0067] Example 5
[0068] The only difference between this embodiment and embodiment 2 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 2kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0069] Example 6
[0070] The only difference between this embodiment and Example 5 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 3kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0071] Example 7
[0072] The only difference between this embodiment and Example 5 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0073] Example 8
[0074] The only difference between this embodiment and Example 7 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, and 0.85kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0075] Example 9
[0076] The only difference between this embodiment and Example 7 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, and 1kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0077] Example 10
[0078] The only difference between this embodiment and embodiment 9 is that the fluorosilicate is sodium fluorosilicate.
[0079] Embodiment 11
[0080] The only difference between this embodiment and Embodiment 9 is that the self-healing inorganic concrete proliferation waterproofing agent includes the following components in mass: 2 kg silane coupling agent, 0.6 kg anhydrous sodium sulfate, 4 kg nano mineral powder, 1 kg potassium fluorosilicate, 0.1 kg basalt fiber and 0.4 kg rust inhibitor.
[0081] In this embodiment, the fiber length of the basalt fiber is 18 mm, and the tensile strength is 3000-4000 MPa; the rust inhibitor is diammine silver hydroxide.
[0082] The preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows:
[0083] 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, 1kg of potassium fluorosilicate, 0.1kg of basalt fiber and 0.4kg of rust inhibitor were put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and a self-healing inorganic concrete proliferation waterproofing agent was obtained after sieving.
[0084] Example 12
[0085] The only difference between this embodiment and embodiment 11 is that the fiber length of the basalt fiber is 12 mm.
[0086] Embodiment 13
[0087] The only difference between this embodiment and Example 11 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, 1kg of potassium fluorosilicate, 0.3kg of basalt fiber, and 0.4kg of rust inhibitor are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0088] Embodiment 14
[0089] The only difference between this embodiment and Example 13 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, 1kg of potassium fluorosilicate, 0.3kg of basalt fiber, and 0.3kg of rust inhibitor are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0090] Embodiment 15
[0091] The only difference between this embodiment and Example 13 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 4kg of nano mineral powder, 1kg of potassium fluorosilicate, 0.3kg of basalt fiber, and 0.2kg of rust inhibitor are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0092] Example 16
[0093] The only difference between this embodiment and embodiment 1 is that this embodiment uses a stirring device.
[0094] The following is combined with Figure 1-2 This embodiment is described in further detail.
[0095] Reference Figure 1The stirring device comprises a frame mechanism 1 and a stirring mechanism 2. The frame mechanism 1 comprises a support base 11, a support column 12 and a traction arm 13. The support column 12 is vertically fixed on the support base 11. The traction arm 13 is arranged at one end of the support column 12 away from the support base 11. The traction arm 13 is in an "L" shape, with one end close to the support column 12 being obliquely fixed on the support column, and the other end away from the support column 12 being parallel to the support column 12. The stirring mechanism 2 comprises a stirring member 3 and a driving member 4. The stirring member 3 is rotatably arranged on the support column 12 and is rotatably connected to one end of the traction arm 13 away from the support column 12; the driving member 4 is installed on the support base 11 and is connected to the stirring member 3 to drive the stirring member 3 to rotate.
[0096] Reference Figure 1 and Figure 2 The stirring member 3 includes a mixing tank 31, a central shaft 32 and a spiral blade 33. The central shaft 32 is arranged horizontally, and one end in the length direction is rotatably connected to the support column 12, and the other end is rotatably connected to the traction arm 13. The mixing tank 31 includes an inlet and outlet tank 311 and a mixing tank 312. The mixing tank 312 is a hollow truncated cone structure. One end of the mixing tube close to the support column 12 is connected to the central shaft 32, and the other end is open and connected to the inlet and outlet tank 311. The inlet and outlet tank 311 is a hollow cylindrical structure with two ends open. The mixing tank 312, the inlet and outlet tank 311, and the central shaft 32 are integrally formed and the central axis coincides. The spiral blade 33 is spirally arranged on the central shaft 32 and is located in the inner cavity of the inlet and outlet tank 311. A plurality of stirring columns 313 are evenly arranged on the inner side wall of the mixing tube.
[0097] Reference Figure 1 and Figure 2 The driving member 4 includes a driving motor 41, a driving gear 42, a gear mounting seat 43 and a mounting gear ring 44. The gear mounting seat 43 is fixed on the supporting base 11, and the driving gear 42 is rotatably mounted on the gear mounting seat 43. The driving motor 41 is mounted on the supporting base 11, and the output end of the driving motor 41 is connected to the driving gear 42 to drive the driving gear 42 to rotate. The mounting gear ring 44 is sleeved on the outer wall of the inlet and outlet tank 311 and is integrally formed with the inlet and outlet tank 311, and the mounting gear ring 44 is meshed and connected with the driving gear 42.
[0098] The implementation principle of a stirring device in an embodiment of the present application is as follows: each raw material component is put into an inlet and outlet tank 311, and the driving motor 41 is started. The driving motor 41 drives the driving gear 42 to rotate forward, and then drives the inlet and outlet tank 311-mixing tank 312-central shaft 32 to rotate forward by installing a gear ring 44. Under the guidance of the spiral blade 33, each raw material component is sent into the mixing tank 312, and the raw material components are fully stirred under the cooperation of multiple stirring columns 313 and the spiral blade 33; when the stirring is completed, adjust the driving motor 41 so that the driving motor 41 drives the driving gear 42 to rotate in the opposite direction, and then drives the inlet and outlet tank 311-mixing tank 312-central shaft 32 to rotate in the opposite direction by installing a gear ring 44. Under the guidance of the spiral blade 33, the raw material inlet and outlet pipe after being mixed evenly is output from the opening at one end away from the mixing tank 312.
[0099] The preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows:
[0100] 1kg of silane coupling agent, 0.2kg of anhydrous sodium sulfate, 2kg of nano mineral powder and 0.7kg of potassium fluorosilicate are put into the inlet and outlet tank 311, and the drive motor 41 is started to make the inlet and outlet tank 311-mixing tank 312-central axis 32 rotate in the forward direction at 250r / min and stir for 25min, and then adjust the drive motor 41 to make the inlet and outlet tank 311-mixing tank 312-central axis 32 rotate in the reverse direction to discharge the material, and obtain the self-healing inorganic concrete proliferation waterproofing agent after screening.
[0101] Comparative Example
[0102] Comparative Example 1
[0103] The only difference between this comparative example and Example 1 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 0.3 kg of silane coupling agent, 0.2 kg of anhydrous sodium sulfate, 2 kg of nano mineral powder, and 0.7 kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0104] Comparative Example 2
[0105] The only difference between this comparative example and Example 1 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 4 kg of silane coupling agent, 0.2 kg of anhydrous sodium sulfate, 2 kg of nano mineral powder, and 0.7 kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0106] Comparative Example 3
[0107] The only difference between this comparative example and Example 2 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.05kg of anhydrous sodium sulfate, 2kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0108] Comparative Example 4
[0109] The only difference between this comparative example and Example 2 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.8kg of anhydrous sodium sulfate, 2kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0110] Comparative Example 5
[0111] The only difference between this comparative example and Example 5 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 1kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0112] Comparative Example 6
[0113] The only difference between this comparative example and Example 5 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 5kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0114] Comparative Example 7
[0115] The only difference between this comparative example and Example 7 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 0.2kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0116] Comparative Example 8
[0117] The only difference between this comparative example and Example 7 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2kg of silane coupling agent, 0.6kg of anhydrous sodium sulfate, 1.5kg of nano mineral powder, and 0.7kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250r / min for 25min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0118] Comparative Example 9
[0119] The only difference between this comparative example and Example 2 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2.2 kg of silane coupling agent, 2 kg of nano mineral powder, and 0.7 kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0120] Comparative Example 10
[0121] The only difference between this comparative example and Example 2 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2.2 kg of anhydrous sodium sulfate, 2 kg of nano mineral powder, and 0.7 kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0122] Comparative Example 11
[0123] The only difference between this comparative example and Example 7 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2 kg of silane coupling agent, 0.6 kg of anhydrous sodium sulfate, and 4.7 kg of nano mineral powder are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0124] Comparative Example 12
[0125] The only difference between this comparative example and Example 7 is that the preparation method of the self-healing inorganic concrete proliferation waterproofing agent is as follows: 2 kg of silane coupling agent, 0.6 kg of anhydrous sodium sulfate, and 4.7 kg of potassium fluorosilicate are put into a GH-5L mixer, stirred at a speed of 250 r / min for 25 min, and the self-healing inorganic concrete proliferation waterproofing agent is obtained after sieving.
[0126] Performance testing
[0127] The self-healing inorganic concrete proliferation waterproofing agent prepared in Example 1-16 and Comparative Example 1-12 was used as a concrete admixture, and the self-healing inorganic concrete proliferation waterproofing agent was mixed with a concrete substrate (cement: sand and gravel aggregate: water = 1:7:1) at a mass ratio of 1:400 to prepare a concrete sample to obtain a test specimen. The test specimen implementation sample 1-16 corresponds to adding the self-healing inorganic concrete proliferation waterproofing agent obtained in Example 1-16, and the test specimen comparison sample 1-12 corresponds to adding the self-healing inorganic concrete proliferation waterproofing agent obtained in Comparative Example 1-12; and the concrete sample without adding the self-healing inorganic concrete proliferation waterproofing agent was used as a reference specimen reference sample, and the following test was performed:
[0128] Test 1: Referring to the testing standards of GB 18445-2012 "Cement-based penetrating crystalline waterproof material" and GB / T 50082-2009 "Standard for test methods of long-term performance and durability of ordinary concrete", the effects of self-healing inorganic concrete proliferation waterproofing agent on concrete's impermeability, self-healing performance, compressive strength and resistance to chloride ion penetration were tested;
[0129] The primary anti-seepage results reflect the effect of the self-healing inorganic concrete proliferation waterproofing agent on improving the concrete's own density and improving the concrete's anti-seepage performance. The secondary anti-seepage results reflect the effect of the self-healing inorganic concrete proliferation waterproofing agent on the self-healing performance of concrete cracks and the anti-seepage performance after self-healing. The compressive strength results reflect the effect of the self-healing inorganic concrete proliferation waterproofing agent on improving the strength of concrete. The results of the chloride ion penetration resistance performance reflect the effect of the self-healing inorganic concrete proliferation waterproofing agent on improving the concrete's own density, improving the concrete's chloride ion penetration resistance performance and durability.
[0130] Test 2: Conduct crack self-repair test to detect the effect of self-healing inorganic concrete proliferation waterproofing agent on the rapid plugging effect of concrete cracks. The size of the mortar specimen for the crack self-repair test is Φ100mm×50mm. Two specimens are formed in each group according to the same mix ratio. The specimen test method is as follows:
[0131] 1. When the reference specimen and the test specimen are cured in the standard curing room for 7 days, take out the specimen, wipe the surface moisture with a dry cloth, and wrap the sealing tape (50 mm wide and 50 μm thick) around the circumference of the specimen for 5 turns;
[0132] 2. Place the splitting fixture on the pressure plate under the mortar pressure tester, and then place the circumferential surface of the specimen wrapped with sealing tape in the fixture so that the specimen is fixed in the middle of the fixture; set the loading speed to 0.1kN / s, start the tester to load, stop loading when cracks appear on the specimen, remove the specimen, and wrap the sealing tape 5 more times along the circumference of the specimen;
[0133] 3. Place the prefabricated crack specimen wrapped with sealing tape into the bottom of a silicone rubber tube with an inner diameter of 100 mm and a height of 200 mm, and then install two stainless steel hoops with a height of 20 mm on the outside of the rubber tube at the same height as the specimen. Tighten the bolts on the hoops firmly to make the side of the specimen in a sealed state;
[0134] 4. Install the silicone rubber tube with the test piece into the test tank. Add 1000mL of water into the rubber tube at one time, and start timing with a timer immediately. When the crack seepage stops, record the time required for the seepage to disappear, which is the water stop time. The water stop time result reflects the reaction time of the self-healing inorganic concrete proliferation waterproofing agent to the self-repair of the cracks after the concrete cracks and seepage.
[0135] Test 3: Conduct mechanical tests to test the effect of self-healing inorganic concrete proliferation waterproofing agent on improving the compressive strength of concrete. The test method is as follows:
[0136] Concrete test blocks were prepared. Six specimens with a size of 10 cm × 10 cm × 10 cm were prepared for each mix ratio. They were cured in a standard curing environment. The compressive strength (28 d) of the specimens was tested at a stress loading rate of 1 mm / min using an electronic servo universal testing machine.
[0137] Test 4: Conduct an electric flux test to detect the effect of the self-healing inorganic concrete proliferation waterproofing agent on improving the concrete's resistance to chloride ion penetration. The test method is as follows:
[0138] Concrete test blocks were prepared. The test used cylindrical test blocks with a bottom diameter of 100mm and a height of 50mm. After the concrete test blocks were cast for 24 hours, they were placed in a standard curing room (temperature of 20±1℃, humidity of 96%) for 28 days. The electric flux test was carried out using a multifunctional concrete durability comprehensive tester. The automatic data collection function was set to record the current every 5 minutes until 6 hours. A current-time relationship graph was drawn based on the recorded data, and the curve was integrated by area to obtain the electric flux (C) passing through the test for 6 hours. Finally, the calculated electric flux was compared with the electric flux of the benchmark group test piece to obtain the electric flux ratio (%).
[0139] The test results are summarized in Table 1.
[0140] Table 1
[0141]
[0142]
[0143] Combining Examples 1-3 and Comparative Examples 1-3 and Table 1, it can be seen that with the increase in the amount of silane coupling agent, the self-repair reaction time of concrete cracks shows a trend of first decreasing and then increasing. Selecting the amount of silane coupling agent within the formula range disclosed in the present application can reduce the penetration of water into the concrete and give the concrete a relatively excellent comprehensive impermeability; when the amount of silane coupling agent is too much or too little, the self-repair time of concrete cracks is long, the cracks are blocked slowly, and the improvement effect of the primary impermeability of concrete, the self-healing performance of concrete cracks, and the secondary impermeability after self-healing is insufficient, the comprehensive impermeability of concrete is poor, and the increase in concrete compressive strength and resistance to chloride ion penetration is not obvious.
[0144] In combination with Example 2, Example 4-5, Comparative Example 3-4 and Table 1, it can be seen that the addition amount of the reaction accelerator is selected within the scope disclosed in the present application, which can significantly improve the primary impermeability of concrete, and the compressive strength and chloride ion penetration resistance of concrete have significant growth, but the reaction accelerator has a relatively unobvious effect on the self-healing performance of concrete cracks and the enhancement effect of the secondary impermeability after self-healing. When the dosage of the reaction accelerator is too much, the primary impermeability of concrete, the self-healing performance of cracks, and the secondary impermeability after self-healing are not significantly improved; when the dosage of the reaction accelerator is too little, the primary impermeability of concrete and the self-healing performance of concrete cracks, the enhancement effect of the secondary impermeability after self-healing and the compressive strength are insufficient, and the self-repair reaction time of concrete cracks is extended, the comprehensive impermeability of concrete is poor, and the growth of chloride ion penetration resistance is not obvious.
[0145] It can be seen from Example 2, Comparative Examples 9-10 and Table 1 that when the reaction accelerator is used in combination with the silane coupling agent, the two act synergistically, and have an excellent effect of promoting the self-healing of concrete in both the early stage of cracking and water seepage and the later stage of continuous repair, thereby further improving the comprehensive anti-seepage performance of concrete.
[0146] It can be seen from Examples 5-7, Comparative Examples 5-6 and Table 1 that the amount of nano-mineral powder added is selected within the formula range disclosed in the present application. As the amount of nano-mineral powder increases, the self-healing performance of concrete cracks, the enhancement effect of the impermeability after self-healing and the resistance to chloride ion penetration are all improved, and the enhancement effect of the primary impermeability and compressive strength of concrete is relatively unobvious. When the amount of the nano-mineral powder mixture is too much, the primary impermeability, crack self-healing performance, impermeability after self-healing, compressive strength and resistance to chloride ion penetration of concrete are not significantly improved; when the amount of the nano-mineral powder mixture is too little, the primary impermeability, concrete crack self-healing performance, secondary impermeability after self-healing, and resistance to chloride ion penetration of concrete are poor, the comprehensive impermeability of concrete is insufficient, and the change in compressive strength is not obvious.
[0147] It can be seen from Examples 7-9, Comparative Examples 7-8 and Table 1 that by increasing the amount of fluorosilicate added within the scope disclosed in the present application, the primary impermeability of concrete, the self-healing performance of cracks, the secondary impermeability after self-healing, the compressive strength and the resistance to chloride ion penetration of concrete are improved. When the amount of fluorosilicate is too much, the primary impermeability of concrete, the self-healing performance of cracks, the secondary impermeability after self-healing, the compressive strength and the resistance to chloride ion penetration of concrete are not significantly improved; when the amount of fluorosilicate is too little, the primary impermeability of concrete and the secondary impermeability after self-healing are poor, and the compressive strength, the self-healing performance of concrete cracks and the resistance to chloride ion penetration do not change significantly.
[0148] It can be seen from Example 7, Comparative Examples 11-12 and Table 1 that the combination of fluorosilicate and nano mineral powder can further improve the comprehensive impermeability, compressive strength and chloride ion penetration resistance of concrete.
[0149] It can be seen from Example 9, Example 11 and Table 1 that adding basalt fiber to the concrete proliferation waterproofing agent can further promote the improvement of the comprehensive impermeability, crack self-healing performance, compressive strength and chloride ion penetration resistance of concrete; and, it can be seen from Examples 11 and 12 that, under the same basalt fiber quality, appropriately increasing the fiber length is beneficial to improving the mechanical properties of concrete.
[0150] It can be seen from Example 11 and Example 13 and Table 1 that when the amount of basalt fiber increases, the mechanical properties of concrete decrease, and the comprehensive impermeability of concrete also decreases. This may be because too much fiber incorporation makes it difficult to evenly disperse the fibers inside the concrete, and introduces a large number of bubbles, resulting in an increase in pores.
[0151] It can be seen from Example 1, Example 16 and Table 1 that the stirring device disclosed in the present application can fully mix and disperse the components of the proliferation waterproofing agent, so that the prepared concrete has better comprehensive anti-seepage performance, crack self-healing performance, compressive strength and resistance to chloride ion penetration.
[0152] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing a self-healing inorganic concrete proliferation waterproofing agent, characterized in that: The waterproofing agent is composed of the following components: Silane coupling agent 2kg, Reaction accelerator 0.6kg, Nano mineral powder 4kg, Fluorosilicate 1kg, Basalt fiber 0.1kg, Rust inhibitor 0.4kg; The reaction accelerator is anhydrous sodium sulfate; The fiber length of the basalt fiber is 18 mm and the tensile strength is 3000-4800 MPa; The rust inhibitor is diammine silver hydroxide; The fluorosilicate is selected from potassium fluorosilicate; The nano mineral powder is a mixture of nano silicon dioxide, nano calcium carbonate and nano clay in a mass ratio of 1:0.9:0.8; The silane coupling agent is silane coupling agent KH550; Nanoclay is nano-scale calcium-based bentonite; The preparation method of the waterproofing agent comprises the following steps: According to the formula, silane coupling agent, fluorosilicate, nano mineral powder, basalt fiber, reaction accelerator and rust inhibitor are put into a stirring device, fully mixed and dispersed to obtain a self-healing inorganic concrete proliferation waterproofing agent; The stirring device comprises a frame mechanism (1) and a stirring mechanism (2); the stirring mechanism (2) comprises a stirring member (3) and a driving member (4); the stirring member (3) is rotatably arranged on the frame mechanism (1); the driving member (4) is mounted on the frame mechanism (1) and connected to the stirring member (3); the driving member (4) is used to drive the stirring member (3) to rotate.
2. The method for preparing the self-healing inorganic concrete proliferation waterproofing agent according to claim 1, characterized in that: The frame mechanism (1) comprises a support base (11), a support column (12) arranged on the support base (11), and a traction arm (13) connected to the support column (12); the stirring member (3) comprises a mixing tank (31), a central shaft (32) and a spiral blade (33); one end of the central shaft (32) is rotatably connected to the support column (12), and the other end is rotatably connected to the traction arm (13); the mixing tank (31) is sleeved on the central shaft (32) and rotates coaxially with the central shaft (32); one end of the mixing tank (31) close to the support column (12) is connected to the central shaft (32), and the other end is open for loading or unloading; the spiral blade (33) is arranged on the central shaft (32) and is located in the inner cavity of the mixing tank (31); the driving member (4) is connected to the outer wall of the mixing tank (31) to drive the mixing tank (31) to rotate.
3. The method for preparing the self-healing inorganic concrete proliferation waterproofing agent according to claim 2, characterized in that: The driving member (4) comprises a driving motor (41), a driving gear (42), a gear mounting seat (43) and a mounting gear ring (44); the driving motor (41) and the gear mounting seat (43) are both arranged on the supporting base (11); the driving gear (42) is mounted on the gear mounting seat (43); and the output end of the driving motor (41) is connected to the driving gear (42); and the mounting gear ring (44) is sleeved on the outer wall of the mixing tank (31) and meshed with the driving gear (42).