A method for separating and recovering antimony from lead-antimony alloy
By performing nine-stage step-by-step temperature-varying gas-liquid phase separation of lead-antimony alloys under low pressure and high temperature conditions, various problems existing in the separation process of lead-antimony alloys in the prior art are solved, and an efficient, safe and environmentally friendly antimony resource is achieved. Recycling improves recycling rate and product purity.
Patent Information
- Application Number
- CN202410071289.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-01-17
AI Technical Summary
The existing lead-antimony alloy separation technology has problems such as large metal backlog, difficulty in handling electrolytes, high energy consumption, large smoke, high equipment requirements, and serious oxidation losses. In most methods, impurities need to be introduced to increase operating costs, making it difficult to achieve high efficiency. Safe and environmentally friendly antimony resource recycling.
The lead-antimal alloy is separated by nine-stage step by step by step by step by step by gas-liquid phase separation by distillation and gas-liquid phase separation. The nine-stage condensation reflux disk and control heating temperature are used to achieve antimony purification. The process is safe and environmentally friendly, and no new impurities are introduced.
The efficient recycling rate of antimony is achieved by reaching more than 99%, the product is highly purified, the process is safe and environmentally friendly, and the raw materials are widely applicable, which avoids the generation of wastewater and waste gas, reduces operating costs, and improves economic benefits.
Smart Images

Figure CN117887980B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for separating and recovering antimony from a lead-antimony alloy, belonging to the technical field of nonferrous metal pyrometallurgy. Background Art
[0002] Antimony is an essential basic raw material for the development of contemporary society, and is mainly used in high-tech fields such as batteries, electronic information, and optoelectronic guidance. Due to the similar physical and chemical properties of lead and antimony, lead-antimony alloys will be generated in the comprehensive recovery process of primary resources (smoke, refining slag, anode mud and other intermediate products) produced by lead and antimony smelting and secondary resources containing lead and antimony (waste babbitt alloy, lead-acid batteries, etc.), resulting in resource accumulation and waste. Therefore, the recycling of lead-antimony alloys is an important way to achieve the regeneration of antimony resources, which has extremely high environmental, economic and social benefits.
[0003] The existing treatment of lead-antimony alloys includes molten salt electrolysis, crystallization, melting and centrifugal segregation. Among them, the molten salt electrolysis method has problems such as large metal backlog, difficult subsequent treatment of electrolyte and anode mud, and high raw material consumption; the vacuum distillation method has problems such as incomplete separation in one distillation, requiring multiple distillations to separate, and high energy consumption; the crystallization method has problems such as large amount of smoke and large amount of manual labor; the melting method has the problem of large amount of slag; the centrifugal segregation method has the problem of high equipment requirements.
[0004] The Chinese patent with publication number CN114807620A discloses a device and method for vacuum vaporization-directional condensation separation of lead-antimony-arsenic ternary alloy, and introduces a specific structure of a vacuum vaporization-directional condensation separation device for lead-antimony-arsenic alloy. The separation of lead-antimony-arsenic, lead-antimony, and antimony-arsenic alloys is achieved by controlling the heating zone, migration zone, and condensation zone of the device by increasing the temperature, solving the problem that lead and antimony are difficult to separate due to "azeotropic" under vacuum conditions, and at the same time, arsenic is recovered separately in a metallic state. The method adopts horizontal furnace directional condensation, and the volatile arsenic will be volatilized to the low temperature section first, but the volatilization mechanism of lead and antimony is similar, and there is only one directional condensation, and the purity of the prepared product is not high, only 98.9wt% of crude metal.
[0005] The Chinese patent with the publication number CN116445740A discloses a method for separating lead-antimony alloys, wherein the lead-antimony alloy melt is subjected to a first stage of condensation treatment at a certain temperature, and then the solid antimony-rich melt is removed and melted, and then subjected to a second stage of condensation treatment, at which the temperature must be higher than the first stage of condensation treatment temperature. According to the above method, the third to tenth stages of condensation treatment with gradually increasing temperatures are sequentially performed, and finally a solid high-antimony alloy is obtained after the tenth stage of condensation treatment. This method can treat lead-antimony alloys with an antimony mass percentage of 11.2 to 95%, and solid-liquid phase separation is achieved based on the solubility difference between the antimony-rich melt and the lead-antimony alloy melt in the solid-liquid phase under the condition of a temperature of 290 to 633°C. However, since the device is in a non-closed system, the melting and condensation effect in the low temperature stage is obvious, but as the temperature stage increases, a large amount of antimony is oxidized to generate antimony white and volatilizes into the air during the actual operation process. Antimony white is a toxic substance and is difficult to collect in an open operation.
[0006] The Chinese patent with publication number CN108823427A discloses a method for separating and recovering lead from lead-antimony alloy, firstly, copper and lead-antimony alloy are mixed according to the mass ratio of antimony in copper and lead-antimony alloy of 1:1-1.2 to obtain a mixture, smelted in an argon atmosphere, and 3 tons of the mixture are melted at 500-600°C for 30-60 minutes to obtain a mixed melt, and finally the obtained mixed melt is vacuum distilled at a pressure of 20-30 Pa and a temperature of 950-1100°C to collect the volatile condensate pure lead and the residual copper-antimony alloy. The above method needs to introduce impurity copper to achieve the separation between lead and antimony, which will increase the operating cost when the processing volume is large.
[0007] The Chinese patent with publication number CN109825719A discloses a method for separating lead-antimony alloys, firstly, the lead-antimony alloy is continuously fed into a rotating supergravity separation reaction chamber through a feeding system, the reactor is started, and the speed regulating motor drives the reactor on the roller to rotate to generate a stable and adjustable supergravity field, and finally, under the combined action of the supergravity field and the temperature field, the atomic diffusion and mass transfer between the lead-antimony alloys are accelerated to achieve continuous separation between the lead-rich liquid and the antimony-rich melt. However, the above method has high requirements on the material of the rotor, and the safety factor of the rotation process cannot be guaranteed.
[0008] The Chinese patent with publication number CN108842069A discloses a method for fire refining of lead-antimony alloy. First, the lead-antimony alloy and pure copper are mixed in a mass ratio of 100:(13-665) to obtain a mixture, and then the mixture is melted at 1060-1070°C under a nitrogen or argon atmosphere. The antimony component and the lead component are separated by utilizing the greater binding force between copper and antimony than between lead and antimony. Then, the difference in melting point between the copper-antimony alloy and lead is utilized to perform crystallization separation, and finally pure lead with antimony removed is obtained. However, the above method also introduces copper to achieve the separation between lead and antimony, which increases the operating cost. Antimony will also be oxidized to form antimony white during the crystallization process, causing environmental pollution. Summary of the invention
[0009] In view of the problems and shortcomings of the above-mentioned existing separation technologies, the present invention provides a method for separating and recovering antimony from lead-antimony alloy. The present invention is a purely physical separation method, the process is safe and environmentally friendly, no new impurities are introduced, and the raw materials have high universality.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] A method for separating and recovering antimony from a lead-antimony alloy, the steps comprising:
[0012] The lead-antimony alloy is distilled under low pressure and high temperature conditions in a molten state to obtain a mixed metal vapor of lead and antimony. The obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and reflux into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation and liquid phase reflux processes are carried out simultaneously; lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage.
[0013] The antimony content in the lead-antimony alloy is 14-99.9%.
[0014] The pressure of the distillation process is 5-15 Pa, the distillation temperature is 800-1100° C., and the insulation time is 6-10 hours.
[0015] The nine-stage step-by-step temperature change gas-liquid phase separation is specifically as follows:
[0016] The heating temperature of the first gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 760-782°C;
[0017] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 740-760°C;
[0018] The heating temperature of the third gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 720-740°C;
[0019] The heating temperature of the fourth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 690-720°C;
[0020] The heating temperature of the fifth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 670-690°C;
[0021] The heating temperature of the sixth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 630-660°C;
[0022] The heating temperature of the seventh gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 600-620°C;
[0023] The heating temperature of the eighth stage of the metal vapor gas-liquid phase separation process and the liquid phase reflux process is 580-600°C;
[0024] The heating temperature of the ninth stage gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 550-580°C.
[0025] The nine-stage step-by-step temperature-changing gas-liquid phase separation is achieved by installing nine-stage condensation reflux plates and controlling the heating temperature.
[0026] The nine sections of condensation reflux plates are arranged in a left-right distribution, and semi-arc-shaped small holes occupying 1 / 4 of the area of the condensation reflux plates are evenly distributed on the first to ninth sections of the condensation reflux plates.
[0027] The lead-antimony alloy obtained from the first to eighth gas-liquid phase separation stages is returned to the distillation process for further purification.
[0028] The antimony content in the purified crude antimony product is above 99%.
[0029] The lead content in the high-lead alloy is 80-86%.
[0030] The beneficial effects of the present invention are:
[0031] (1) The present invention is a pure physical separation method, no waste water or waste gas is generated during the operation, and it is safe and environmentally friendly;
[0032] (2) The lead-antimony separation process of the present invention does not introduce any impurities;
[0033] (3) The raw material of the present invention has high universality and can process lead-antimony alloys with antimony contents of 14 to 99.9%;
[0034] (4) The distillation, gas-liquid phase separation and liquid phase reflux processes of the present invention are carried out simultaneously;
[0035] (5) The recovery rate of antimony in the present invention is relatively high, reaching more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a process flow chart of the present invention;
[0037] Figure 2 It is a schematic diagram of the principle of the present invention;
[0038] Figure 3 This is the XRD and chemical composition analysis sheet of the crude antimony prepared in Example 1 of the present invention;
[0039] Figure 4 This is a physical picture of the crude antimony prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0041] Example 1
[0042] like Figures 1 to 2 As shown, the method for separating and recovering antimony from lead-antimony alloy comprises the following steps:
[0043] A lead-antimony alloy containing 75% lead and 25% antimony is distilled at 10Pa and 1100°C for 8h, and the obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and flow back into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation, and liquid phase reflux processes are carried out simultaneously; a lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage;
[0044] The nine stages of step-by-step temperature change for gas-liquid separation are as follows:
[0045] The heating temperature of the first gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 765°C;
[0046] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 745°C;
[0047] The heating temperature of the third gas-liquid phase separation process and liquid phase reflux process of metal vapor is 725°C;
[0048] The heating temperature of the fourth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 695°C;
[0049] The heating temperature of the fifth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 670°C;
[0050] The heating temperature of the sixth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 640°C;
[0051] The heating temperature of the seventh gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 605°C;
[0052] The heating temperature of the eighth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 595°C;
[0053] The heating temperature of the ninth stage gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 565°C.
[0054] The nine-stage step-by-step temperature-changing gas-liquid phase separation is achieved by installing a nine-stage condensing reflux plate and controlling the heating temperature;
[0055] The nine sections of condensation reflux plates are arranged in a left-right distribution, and semi-arc-shaped small holes occupying 1 / 4 of the area of the condensation reflux plates are evenly distributed on the first to ninth sections of the condensation reflux plates.
[0056] The XRD analysis diagram of the crude antimony prepared in this example is as follows Figure 3 As shown; the crude antimony prepared in this example is shown in Figure 4 As shown. Figure 3 and Figure 4 It can be seen that crude antimony is prepared in the present invention.
[0057] The experimental results of this embodiment are shown in Table 1.
[0058] Table 1 Experimental results of Example 1
[0059]
[0060] As can be seen from Table 1, the crude antimony prepared by the present invention has an Sb content of 99.53% and a Pb content of 0.47%. The antimony recovery rate of the present invention reaches more than 99%. Compared with the antimony recovery rate of 98% in the patent application with publication number CN116445740A, the recovery effect of the present invention is significantly improved, and the economic benefit is significantly increased. At the same time, the present invention is carried out under vacuum conditions, which can effectively prevent the occurrence of product oxidation, and can process lead-antimony alloys with antimony contents of 14 to 99.9%. The material adaptability is wide, which is more conducive to the industrialization of vacuum segmented condensation of lead-antimony alloys.
[0061] Example 2
[0062] like Figures 1 to 2 As shown, the method for separating and recovering antimony from lead-antimony alloy comprises the following steps:
[0063] A lead-antimony alloy containing 25% lead and 75% antimony is distilled at 10Pa and 1000°C for 10 hours, and the obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and flow back into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation, and liquid phase reflux processes are carried out simultaneously; a lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage;
[0064] The nine-stage step-by-step temperature change gas-liquid phase separation with gradually decreasing temperature is as follows:
[0065] The heating temperature of the first gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 775°C;
[0066] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 755°C;
[0067] The heating temperature of the third gas-liquid phase separation process and liquid phase reflux process of metal vapor is 735°C;
[0068] The heating temperature of the fourth stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 705°C;
[0069] The heating temperature of the fifth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 675°C;
[0070] The heating temperature of the sixth stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 635°C;
[0071] The heating temperature of the seventh gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 620°C;
[0072] The heating temperature of the eighth stage of the metal vapor gas-liquid phase separation process and the liquid phase reflux process is 585°C;
[0073] The heating temperature of the ninth stage gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 555°C.
[0074] The nine-stage step-by-step temperature-changing gas-liquid phase separation with gradually decreasing temperature is achieved by installing a nine-stage condensing reflux plate and controlling the heating temperature;
[0075] The nine sections of condensation reflux plates are arranged in a left-right distribution, and semi-arc-shaped small holes occupying 1 / 4 of the area of the condensation reflux plates are evenly distributed on the first to ninth sections of the condensation reflux plates.
[0076] The experimental results of this embodiment are shown in Table 2.
[0077] Table 2 Experimental results of Example 2
[0078]
[0079] It can be seen from Table 2 that the crude antimony prepared by the present invention contains 99.39% Sb and 0.61% Pb.
[0080] Example 3
[0081] like Figures 1 to 2 As shown, the method for separating and recovering antimony from lead-antimony alloy comprises the following steps:
[0082] A lead-antimony alloy containing 50% lead and 50% antimony is distilled at 5Pa and 900°C for 8h, and the obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and flow back into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation, and liquid phase reflux processes are carried out simultaneously; a lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage;
[0083] The nine-stage gas-liquid phase separation with gradually decreasing temperature is as follows:
[0084] The heating temperature of the first gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 780°C;
[0085] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 760°C;
[0086] The heating temperature of the third gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 740°C;
[0087] The heating temperature of the fourth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 710°C;
[0088] The heating temperature of the fifth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 680°C;
[0089] The heating temperature of the sixth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 640°C;
[0090] The heating temperature of the seventh gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 600°C;
[0091] The heating temperature of the eighth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 580°C;
[0092] The heating temperature of the ninth stage gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 560°C.
[0093] The nine-stage gas-liquid phase separation with gradually decreasing temperature is realized by installing nine-stage condensation reflux plates and controlling the heating temperature;
[0094] The nine sections of condensation reflux plates are arranged in a left-right distribution, and semi-arc-shaped small holes occupying 1 / 4 of the area of the condensation reflux plates are evenly distributed on the first to ninth sections of the condensation reflux plates.
[0095] The experimental results of this embodiment are shown in Table 3.
[0096] Table 3 Experimental results of Example 3
[0097]
[0098]
[0099] It can be seen from Table 3 that the crude antimony prepared by the present invention contains 99.25% Sb and 0.75% Pb.
[0100] Example 4
[0101] like Figures 1 to 2 As shown, the method for separating and recovering antimony from lead-antimony alloy comprises the following steps:
[0102] A lead-antimony alloy containing 5% lead and 95% antimony is distilled at 15Pa and 800°C for 7h, and the obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and flow back into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation, and liquid phase reflux processes are carried out simultaneously; a lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage;
[0103] The nine-stage gas-liquid phase separation with gradually decreasing temperature is as follows:
[0104] The heating temperature of the first gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 770°C;
[0105] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 750°C;
[0106] The heating temperature of the third gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 730°C;
[0107] The heating temperature of the fourth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 710°C;
[0108] The heating temperature of the fifth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 670°C;
[0109] The heating temperature of the sixth stage of the metal vapor gas-liquid phase separation process and the liquid phase reflux process is 630°C;
[0110] The heating temperature of the seventh gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 615°C;
[0111] The heating temperature of the eighth stage of the metal vapor gas-liquid phase separation process and the liquid phase reflux process is 585°C;
[0112] The heating temperature of the ninth stage gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 550°C.
[0113] The nine-stage gas-liquid phase separation with gradually decreasing temperature is realized by installing nine-stage condensation reflux plates and controlling the heating temperature;
[0114] The nine sections of condensation reflux plates are arranged in a left-right distribution, and semi-arc-shaped small holes occupying 1 / 4 of the area of the condensation reflux plates are evenly distributed on the first to ninth sections of the condensation reflux plates.
[0115] The experimental results of this embodiment are shown in Table 4.
[0116] Table 4 Experimental results of Example 4
[0117]
[0118] It can be seen from Table 4 that the crude antimony prepared by the present invention contains 99.01% Sb and 0.99% Pb.
[0119] Comparative Example 1
[0120] A method for separating and recovering antimony from lead-antimony alloy comprises the following steps:
[0121] A lead-antimony alloy containing 5% lead and 95% antimony is distilled at 10Pa and 1200°C for 8h, and the obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and flow back into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation, and liquid phase reflux processes are carried out simultaneously; a lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage;
[0122] The nine-stage gas-liquid phase separation with gradually decreasing temperature is as follows:
[0123] The heating temperature of the first gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 750°C;
[0124] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 725°C;
[0125] The heating temperature of the third gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 700°C;
[0126] The heating temperature of the fourth stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 670°C;
[0127] The heating temperature of the fifth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 645°C;
[0128] The heating temperature of the sixth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 610°C;
[0129] The heating temperature of the seventh gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 580°C;
[0130] The heating temperature of the eighth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 545°C;
[0131] The heating temperature of the ninth stage gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 530°C.
[0132] The experimental results of this comparative example 1 are shown in Table 5.
[0133] Table 5 Experimental results of comparative example 1
[0134]
[0135] As can be seen from Table 5, ten stages of gas-liquid phase separation with gradually decreasing temperature were carried out, but without the specific temperature of the present invention, there was no way to obtain a crude antimony product. The lead content in the obtained lead-antimony alloy product was 29.52%, and the separation effect was poor.
[0136] Comparative Example 2
[0137] A method for separating and recovering antimony from lead-antimony alloy comprises the following steps:
[0138] A lead-antimony alloy containing 5% lead and 95% antimony is distilled at 10Pa and 1100°C for 8h, and the obtained metal vapor is subjected to five-stage step-by-step temperature-changing gas-liquid phase separation. The liquid phase obtained after separation will take away part of the lead in the metal vapor and flow back into the lead-antimony alloy melt for distillation and gas-liquid phase separation again. The antimony content of the obtained gas phase gradually increases, and antimony purification can be achieved. In this process, distillation, gas-liquid phase separation, and liquid phase reflux processes are carried out simultaneously; a lead-antimony alloy is obtained in the first to fifth gas-liquid phase separation stages, and a high-lead alloy is obtained in the distillation stage;
[0139] The five-stage gas-liquid phase separation with gradually decreasing temperature is as follows:
[0140] The heating temperature of the first gas-liquid phase separation process of the metal vapor and the liquid phase reflux process is 765°C;
[0141] The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 745°C;
[0142] The heating temperature of the third gas-liquid phase separation process and liquid phase reflux process of metal vapor is 725°C;
[0143] The heating temperature of the fourth gas-liquid phase separation process and liquid phase reflux process of the metal vapor is 695°C;
[0144] The heating temperature of the fifth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 675°C.
[0145] The experimental results of this comparative example 2 are shown in Table 6.
[0146] Table 6 Experimental results of comparative example 2
[0147]
[0148] As can be seen from Table 6, without the ten-stage gas-liquid phase separation with gradually decreasing temperature, it is impossible to obtain a crude antimony product. The lead content in the obtained lead-antimony alloy product is 30.58%, and the separation effect is also poor.
[0149] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for separating and recovering antimony from a lead-antimony alloy, comprising the following steps: The lead-antimony alloy is distilled under low pressure and high temperature conditions to obtain mixed metal vapor of lead and antimony, the obtained metal vapor is subjected to nine-stage step-by-step temperature-changing gas-liquid phase separation, the liquid phase obtained after separation is refluxed into the lead-antimony alloy melt for distillation and gas-liquid phase separation again, during which the distillation, gas-liquid phase separation and liquid phase reflux processes are carried out simultaneously; the lead-antimony alloy is obtained in the first to eighth gas-liquid phase separation stages, crude antimony is obtained in the ninth gas-liquid phase separation stage, and a high-lead alloy is obtained in the distillation stage; The distillation process pressure is 5~15Pa, the distillation temperature is 800~1100℃, and the insulation time is 6~10h; The nine-stage step-by-step temperature change gas-liquid phase separation is specifically as follows: The heating temperature of the first gas-liquid phase separation process of metal vapor and the liquid phase reflux process is 760~782℃; The heating temperature of the second gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 740~760℃; The heating temperature of the third stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 720~740℃; The heating temperature of the fourth stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 690~720℃; The heating temperature of the fifth gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 670~690℃; The heating temperature of the sixth stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 630~660℃; The heating temperature of the seventh gas-liquid phase separation process and the liquid phase reflux process of the metal vapor is 600~620℃; The heating temperature of the eighth stage of metal vapor gas-liquid phase separation process and liquid phase reflux process is 580~600℃; The heating temperature of the ninth stage of the metal vapor gas-liquid phase separation process and the liquid phase reflux process is 550~580℃; The nine-stage step-by-step temperature-changing gas-liquid phase separation is achieved by installing nine-stage condensation reflux plates and controlling the heating temperature; The nine sections of condensation reflux plates are arranged in a left-right distribution, and semi-arc-shaped small holes occupying 1 / 4 of the area of the condensation reflux plates are evenly distributed on the first to ninth sections of the condensation reflux plates.
2. The method for separating and recovering antimony from lead-antimony alloy according to claim 1, characterized in that: The antimony content in the lead-antimony alloy is 14-99.9%.
3. The method for separating and recovering antimony from lead-antimony alloy according to claim 1, characterized in that: The lead-antimony alloy obtained from the first to eighth gas-liquid phase separation stages is returned to the distillation process for further purification.
4. The method for separating and recovering antimony from lead-antimony alloy according to claim 1, characterized in that: The antimony content in the crude antimony is more than 99%.
5. The method for separating and recovering antimony from lead-antimony alloy according to claim 1, characterized in that: The lead content in the high-lead alloy is 80-86%.
Citation Information
Patent Citations
Method of separating and recovering lead from lead-antimony alloy
CN108823427A
Method for fire refining of lead-antimony alloy
CN108842069A
Method and device for separating lead-antimony alloys by supergravity
CN109825719A
Vacuum gasification-directional condensation separation equipment and method for lead-antimony-arsenic ternary alloy
CN114807620A
Separation method of lead-antimony alloy
CN116445740A